Rare earth aluminum alloy high-temperature-resistant cable and preparation method thereof

By adding rare earth elements and titanium, praseodymium, neodymium and other elements to the aluminum alloy cable, and setting a refractory layer and filler outside the cable, the problems of low tensile strength and poor high temperature stability of the aluminum alloy cable are solved, which significantly improves the cable Creep resistance and service life.

CN118969390APending Publication Date: 2024-11-15GUANGDONG TENGYUETONG CABLE CO LTD

Patent Information

Application Number
CN202411038888.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The tensile strength of aluminum alloy cables is low and the high temperature stability is poor, which affects the normal use of the cable.

Method used

Rare earth aluminum alloy materials are used, and elements such as titanium, praseodymium, neodymium are added to refine the grains, improve tensile strength and high temperature performance, and mica refractory layer, ceramic silicone rubber filler and low-smoke halogen-free external protection are installed outside the cable. The cable is enhanced with flame retardant and high temperature resistance.

Benefits of technology

The tensile strength, toughness and conductivity of aluminum alloy cables are improved, the high temperature stability and service life are enhanced, and the creep resistance of the cable is significantly improved, with a service life of no less than 45 years.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969390A_ABST
    Figure CN118969390A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth aluminum alloy high-temperature-resistant cable and a preparation method thereof, and belongs to the technical field of aluminum alloy cables. The aluminum alloy wire is characterized by comprising an aluminum alloy monofilament, and the aluminum alloy monofilament comprises, by mass, 1.0%-2.0% of titanium, 0.15%-1.5% of copper, 0.03%-0.10% of manganese, 0.03%-0.08% of zirconium, 0.2%-1.5% of iron, 0.02%-0.08% of nickel, 0.03%-0.09% of cobalt, 0.15%-3.0% of rare earth, 0.3%-0.8% of yttrium barium copper oxide, less than or equal to 0.3% of impurities and the balance aluminum. The rare earth comprises the following components in percentage by mass: 0.02 to 1.2 percent of praseodymium, 0.03 to 0.5 percent of lanthanum, 0.03 to 0.5 percent of cerium, 0.03 to 0.5 percent of neodymium and 0.03 to 0.5 percent of yttrium. The invention further discloses a preparation method of the rare earth aluminum alloy high-temperature-resistant cable. By the adoption of the rare earth aluminum alloy high-temperature-resistant cable and the preparation method thereof, the problems that an existing aluminum alloy cable is low in tensile strength and poor in high-temperature stability can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy cables, and in particular to a rare earth aluminum alloy high temperature resistant cable and a preparation method thereof. Background Art

[0002] With the rapid development of my country's national economy, cables, as the main carrier of power transmission, have been used in more and more occasions, and the requirements for cables are getting higher and higher, especially in schools, hospitals, real estate, large entertainment venues and other projects, which have stricter fire protection requirements and higher fire resistance requirements for cables. Aluminum alloy cables have been widely used because of their light weight and low price. However, the high temperature resistance of aluminum alloy cables is relatively poor. Under high temperature conditions, aluminum alloy cables are easily deformed, affecting the normal use of cables.

[0003] The existing patent CN202010721123.X discloses a rare earth high-speed iron aluminum alloy fireproof cable, including a rare earth high-speed iron aluminum alloy conductor and a protective layer, at least two rare earth high-speed iron aluminum alloy conductors are arranged inside the protective layer; a fireproof layer and a first insulating layer are arranged on the outside of the rare earth high-speed iron aluminum alloy conductor, the fireproof layer is located between the rare earth high-speed iron aluminum alloy conductor and the first insulating layer, and a second insulating layer is arranged between the first insulating layer and the protective layer; the protective layer is sequentially provided with concentric flame retardant layers and sheaths from the inside to the outside, the sheath is located outside the flame retardant layer, and a second insulating layer is arranged between the flame retardant layer and the first insulating layer. The rare earth high iron aluminum alloy monofilament includes the following components by mass percentage: iron 1.0-1.5%, silicon 0.03-0.08%, copper 0.02-0.08%, manganese 0.02-0.08%, magnesium 0.01-0.05%, titanium 0.01-0.08%, zirconium 0.01-0.08%, chromium 0.05-0.1%, strontium 0.01-0.05%, rare earth 0.8-1.5%, the total impurity content ≤ 0.1%, and the balance aluminum. The fireproof performance of the cable in the above patent mainly depends on the fireproof structure of the cable outer coating, the tensile strength of the cable is relatively low, and the creep resistance of the cable is poor, which affects the stability of the cable under high temperature conditions. Summary of the invention

[0004] The purpose of the present invention is to provide a rare earth aluminum alloy high temperature resistant cable and a preparation method thereof, so as to solve the problems of relatively low tensile strength and poor high temperature stability of existing aluminum alloy cables.

[0005] To achieve the above-mentioned purpose, the present invention provides a rare earth aluminum alloy high temperature resistant cable, comprising an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in mass percentage: titanium 1.0%-2.0%, copper 0.15%-1.5%, manganese 0.03%-0.10%, zirconium 0.03%-0.08%, iron 0.2%-1.5%, nickel 0.02%-0.08%, cobalt 0.03%-0.09%, rare earth 0.15%-2.5%, yttrium 0.03%-0.5%, yttrium barium copper oxide 0.3%-0.8%, the total impurity content ≤0.3%, and the balance aluminum.

[0006] Preferably, the rare earth includes the following components in mass percentage: praseodymium 0.02%-1.2%, lanthanum 0.03%-0.5%, cerium 0.03%-0.5%, neodymium 0.03%-0.5%.

[0007] Preferably, it includes a rare earth aluminum alloy conductor, which is formed by twisting aluminum alloy monofilaments, a fire-resistant layer is arranged on the outside of the aluminum alloy conductor, an insulating layer is arranged on the outside of the fire-resistant layer, a glass fiber tape is wound on the outside of the insulating layer, at least one rare earth aluminum alloy conductor is arranged on the inside of the glass fiber tape, a high-temperature resistant filler is arranged between the insulating layer and the glass fiber tape, an inner sheath layer is arranged on the outside of the glass fiber tape, an outer sheath layer is arranged on the outside of the inner sheath layer, and an armor layer is arranged between the inner sheath layer and the outer sheath layer.

[0008] Preferably, the fire-resistant layer is a mica tape layer, the insulating layer is a polytrifluorochloroethylene layer, the high-temperature resistant filler is ceramic silicone rubber, the armor layer is a galvanized steel tape layer, and the outer sheath layer is a low-smoke halogen-free layer.

[0009] The method for preparing the rare earth aluminum alloy high temperature resistant cable comprises the following steps:

[0010] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition;

[0011] S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid;

[0012] S3, smelting, adding weighed raw materials and low-oxygen hydrogenated dehydrogenated titanium powder into aluminum liquid for melting, adding grain refiner into the aluminum liquid, smelting, refining and degassing, melting evenly and then keeping warm to obtain rare earth aluminum alloy liquid;

[0013] S4, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars;

[0014] S5, rolling, rolling the rare earth aluminum alloy strip through a rolling mill to form a rare earth aluminum alloy rod with a diameter of Φ9.0 mm;

[0015] S6, drawing, using a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical aluminum alloy monofilament, and twisting the aluminum alloy monofilament into a rare earth aluminum alloy conductor on a frame-type stranding machine using a special-shaped stranding die;

[0016] S7, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing;

[0017] S8, insulation, cabling, sheathing, after cooling, wrap a layer of mica tape on the outside of the rare earth aluminum alloy conductor to form a fire-resistant layer, and extrude the insulation layer with polytrifluorochloroethylene; fill the insulation layer with ceramic silicone rubber high-temperature resistant filler, and after filling, wrap it with glass fiber tape to form a cable and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with low-smoke halogen-free material to form a cable.

[0018] Preferably, in S2, the purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 750°C-800°C.

[0019] Preferably, in S3, the grain refiner is Al-5Ti-B refiner, and the mass percentage of grain refinement is 0.5%-1%.

[0020] Preferably, in S7, the annealing temperature is 300°C±10°C, and the annealing time is 6 hours to 9 hours.

[0021] The aluminum alloy monofilament prepared by the above-mentioned preparation method of rare earth aluminum alloy high temperature resistant cable has an elongation of ≥35% and a tensile strength of 135N / mm 2 -170N / mm 2 , 90° bending times more than 30 times, DC resistivity ≤0.0278Ω / m at 20℃, conductivity 62%-63%, bending radius 7D-12D, compared with copper cable, its rebound performance is reduced by 45%, compared with aluminum core cable, its creep resistance is increased by 350%, and its service life is not less than 45 years.

[0022] The advantages and positive effects of the rare earth aluminum alloy high temperature resistant cable and the preparation method thereof of the present invention are:

[0023] 1. The present invention adds more rare earth elements to the aluminum alloy. The rare earth elements can modify the aluminum alloy, refine the grains of the aluminum alloy, and improve the structure of the aluminum alloy, thereby improving the tensile strength, toughness and conductivity of the aluminum alloy.

[0024] 2. The rare earth elements of the present invention contain not only lanthanum and cerium for refining the aluminum alloy, but also praseodymium and neodymium. In addition to being able to refine the grains of the aluminum alloy, praseodymium and neodymium can also improve the high temperature performance of the aluminum alloy, and improve the mechanical properties and stability of the aluminum alloy under high temperature conditions.

[0025] 3. The present invention adds yttrium barium copper oxide to the aluminum alloy, and yttrium barium copper oxide can improve the electrical conductivity of the aluminum alloy cable at high temperatures.

[0026] 4. The present invention adds titanium to the aluminum alloy, which can hinder the precipitation of needle-shaped or flaky second phases in the aluminum alloy, promote the dispersion precipitation of fine strengthening particles, and improve the strength of the aluminum alloy. In addition, titanium can improve the heat resistance of the aluminum alloy and improve the high-temperature stability of the aluminum alloy.

[0027] 5. The present invention arranges a mica fire-resistant layer on the outside of the rare earth aluminum alloy conductor, fills it with high-temperature resistant filler, and uses polytrifluorochloroethylene for insulation. The outermost layer uses a low-smoke halogen-free outer sheath layer, which improves the flame retardant and high-temperature resistance of the cable, and improves the corrosion resistance, strong alkali resistance and strong oxidation resistance of the cable.

[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of a cable cross-section structure according to an embodiment of the present invention;

[0030] Figure 2 is a flow chart of an embodiment of the present invention.

[0031] Reference numerals

[0032] 1. Rare earth aluminum alloy conductor; 2. Refractory layer; 3. Insulation layer; 4. High temperature resistant filler; 5. Glass fiber tape; 6. Inner sheath layer; 7. Armor layer; 8. Outer sheath layer. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0034] Unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0035] A rare earth aluminum alloy high temperature resistant cable comprises an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in mass percentage: 1.0%-2.0% titanium, 0.15%-1.5% copper, 0.03%-0.10% manganese, 0.03%-0.08% zirconium, 0.2%-1.5% iron, 0.02%-0.08% nickel, 0.03%-0.09% cobalt, 0.15%-2.5% rare earth, 0.03%-0.5% yttrium, 0.3%-0.8% yttrium barium copper oxide, the total impurity content is ≤0.3%, and the balance is aluminum.

[0036] The rare earth includes the following components in percentage by mass: praseodymium 0.02-1.2%, lanthanum 0.03-0.5%, cerium 0.03-0.5%, and neodymium 0.03-0.5%.

[0037] like Figure 1 As shown. The rare earth aluminum alloy high temperature resistant cable comprises a rare earth aluminum alloy conductor, which is made of aluminum alloy monofilaments. The aluminum alloy monofilament is an elliptical structure, and the elliptical aluminum alloy monofilament allows the aluminum alloy monofilaments to be tightly combined together, thereby increasing the number of aluminum alloy monofilaments per unit area. A fire-resistant layer is arranged on the outside of the aluminum alloy conductor, and the fire-resistant layer is a mica tape layer. The mica tape can maintain structural stability under high temperature environment, play a role in isolating the spread of flames and heat conduction, and has high temperature resistance and insulation. The mica tape layer is arranged on the outside of the aluminum alloy conductor to protect the aluminum alloy conductor and reduce the influence of high temperature on the performance of the aluminum alloy conductor. An insulating layer is arranged on the outside of the fire-resistant layer, and the insulating layer is a polytrifluorochloroethylene layer. Polytrifluorochloroethylene has excellent chemical stability and heat resistance, which is beneficial to improving the heat resistance of the cable. A glass fiber tape is wound on the outside of the insulating layer, and the rare earth aluminum alloy conductor is wrapped and wound together by the glass fiber tape. The glass fiber tape has a relatively good supporting effect on the one hand, and has good high temperature resistance on the other hand, which is beneficial to improving the high temperature resistance of the cable. A high temperature resistant filler is arranged between the insulating layer and the glass fiber tape, and the high temperature resistant filler is ceramic silicone rubber. An inner sheath layer is arranged outside the glass fiber tape, an outer sheath layer is arranged outside the inner sheath layer, and an armor layer is arranged between the inner sheath layer and the outer sheath layer. The armor layer is a galvanized steel tape layer, and the outer sheath layer is a low smoke zero halogen layer. Both ceramic silicone rubber and low smoke zero halogen layer are conducive to improving the heat resistance and fire resistance of the cable.

[0038] like Figure 2 The method for preparing the rare earth aluminum alloy high temperature resistant cable comprises the following steps:

[0039] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0040] S2. Melting the aluminum ingot: Put the aluminum ingot into a melting furnace for melting, and keep it warm after melting to obtain aluminum liquid. The purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 750℃-800℃.

[0041] S3, smelting, adding weighed raw materials and low-oxygen hydrogenated dehydrogenated titanium powder into aluminum liquid for melting, adding grain refiner into the aluminum liquid, smelting, refining and degassing, and keeping warm after uniform melting to obtain rare earth aluminum alloy liquid.

[0042] The grain refiner is Al-5Ti-B refiner, and the mass percentage of grain refinement is 0.5%-1%.

[0043] S4, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0044] S5. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0045] S6. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0046] S7, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0047] The annealing temperature is 300°C ± 10°C, and the annealing time is 6 hours to 9 hours.

[0048] S8, insulation, cabling, sheathing, after cooling, wrap a layer of mica tape on the outside of the rare earth aluminum alloy conductor to form a fire-resistant layer, and extrude the insulation layer with polytrifluorochloroethylene; fill the insulation layer with ceramic silicone rubber high-temperature resistant filler, and after filling, wrap it with glass fiber tape to form a cable and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with low-smoke halogen-free material to form a cable.

[0049] Example 1

[0050] A rare earth aluminum alloy high temperature resistant cable comprises an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in percentage by mass: 1.8% titanium, 1.2% copper, 0.08% manganese, 0.05% zirconium, 1.0% iron, 0.08% nickel, 0.04% cobalt, 1.8% rare earth, 0.2% yttrium, 0.3% yttrium barium copper oxide, the total impurity content ≤0.3%, and the remainder aluminum.

[0051] The rare earth includes the following components in percentage by mass: praseodymium 1.0%, lanthanum 0.4%, cerium 0.2%, and neodymium 0.2%.

[0052] The method for preparing a rare earth aluminum alloy high temperature resistant cable comprises the following steps:

[0053] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0054] S2. Melting the aluminum ingot: Put the aluminum ingot into a melting furnace for melting, keep the temperature after melting, and obtain aluminum liquid. The purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 750℃.

[0055] S3, smelting, adding weighed raw materials and low-oxygen hydrogenated dehydrogenated titanium powder into aluminum liquid for melting, adding grain refiner into the aluminum liquid, smelting, refining and degassing, and keeping warm after uniform melting to obtain rare earth aluminum alloy liquid.

[0056] The grain refiner is Al-5Ti-B refiner, and the mass percentage of grain refinement is 0.8%.

[0057] S4, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0058] S5. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0059] S6. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0060] S7, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0061] The annealing temperature is 300°C ± 10°C, and the annealing time is 7 hours.

[0062] S8, insulation, cabling, sheathing, after cooling, wrap a layer of mica tape on the outside of the rare earth aluminum alloy conductor to form a fire-resistant layer, and extrude the insulation layer with polytrifluorochloroethylene; fill the insulation layer with ceramic silicone rubber high-temperature resistant filler, and after filling, wrap it with glass fiber tape to form a cable and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with low-smoke halogen-free material to form a cable.

[0063] Example 2

[0064] A rare earth aluminum alloy high temperature resistant cable comprises an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in mass percentage: 1.5% titanium, 0.6% copper, 0.05% manganese, 0.08% zirconium, 1.2% iron, 0.04% nickel, 0.08% cobalt, 2.3% rare earth, 0.5% yttrium, 0.5% yttrium barium copper oxide, the total impurity content is ≤0.3%, and the balance is aluminum.

[0065] The rare earth includes the following components in percentage by mass: praseodymium 1.2%, lanthanum 0.3%, cerium 0.5%, and neodymium 0.3%.

[0066] The method for preparing a rare earth aluminum alloy high temperature resistant cable comprises the following steps:

[0067] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0068] S2, melting the aluminum ingot, putting the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid. The purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 780℃.

[0069] S3, smelting, adding weighed raw materials and low-oxygen hydrogenated dehydrogenated titanium powder into aluminum liquid for melting, adding grain refiner into the aluminum liquid, smelting, refining and degassing, and keeping warm after uniform melting to obtain rare earth aluminum alloy liquid.

[0070] The grain refiner is Al-5Ti-B refiner, and the mass percentage of grain refinement is 1%.

[0071] S4, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0072] S5. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0073] S6. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0074] S7, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0075] The annealing temperature is 300°C ± 10°C, and the annealing time is 8 hours.

[0076] S8, insulation, cabling, sheathing, after cooling, wrap a layer of mica tape on the outside of the rare earth aluminum alloy conductor to form a fire-resistant layer, and extrude the insulation layer with polytrifluorochloroethylene; fill the insulation layer with ceramic silicone rubber high-temperature resistant filler, and after filling, wrap it with glass fiber tape to form a cable and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with low-smoke halogen-free material to form a cable.

[0077] Example 3

[0078] A rare earth aluminum alloy high temperature resistant cable comprises an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in percentage by mass: 1.2% titanium, 0.2% copper, 0.08% manganese, 0.05% zirconium, 0.4% iron, 0.03% nickel, 0.09% cobalt, 1.2% rare earth, 0.4% yttrium, 0.7% yttrium barium copper oxide, the total impurity content is ≤0.3%, and the remainder is aluminum.

[0079] The rare earth includes the following components in percentage by mass: praseodymium 0.4%, lanthanum 0.4%, cerium 0.3%, and neodymium 0.1%.

[0080] The method for preparing a rare earth aluminum alloy high temperature resistant cable comprises the following steps:

[0081] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0082] S2. Melting the aluminum ingot: placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid. The purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 760°C.

[0083] S3, smelting, adding weighed raw materials and low-oxygen hydrogenated dehydrogenated titanium powder into aluminum liquid for melting, adding grain refiner into the aluminum liquid, smelting, refining and degassing, and keeping warm after uniform melting to obtain rare earth aluminum alloy liquid.

[0084] The grain refiner is Al-5Ti-B refiner, and the mass percentage of grain refinement is 0.8%.

[0085] S4, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0086] S5. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0087] S6. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0088] S7, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0089] The annealing temperature is 300°C ± 10°C, and the annealing time is 6 hours.

[0090] S8, insulation, cabling, sheathing, after cooling, wrap a layer of mica tape on the outside of the rare earth aluminum alloy conductor to form a fire-resistant layer, and extrude the insulation layer with polytrifluorochloroethylene; fill the insulation layer with ceramic silicone rubber high-temperature resistant filler, and after filling, wrap it with glass fiber tape to form a cable and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with low-smoke halogen-free material to form a cable.

[0091] The properties of the aluminum alloy monofilaments prepared in Examples 1-3 were tested, and the test results are shown in Table 1.

[0092] Table 1 Properties of aluminum alloy monofilaments prepared in Examples 1-3

[0093]

[0094]

[0095] The cable bending radius obtained in Examples 1-3 is 7D-12D, the cable rebound performance is reduced by 45% compared with copper cables, the creep resistance is increased by 350% compared with aluminum core cables, and the service life is not less than 45 years, which improves the service life and creep resistance of the cable and has very good high temperature stability.

[0096] Therefore, the rare earth aluminum alloy high temperature resistant cable and the preparation method thereof described in the present invention can solve the problems of relatively low tensile strength and poor high temperature stability of existing aluminum alloy cables.

[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A rare earth aluminum alloy high temperature resistant cable, characterized in that: Including aluminum alloy monofilament, the aluminum alloy monofilament includes the following components in mass percentage: titanium 1.0%-2.0%, copper 0.15%-1.5%, manganese 0.03%-0.10%, zirconium 0.03%-0.08%, iron 0.2%-1.5%, nickel 0.02%-0.08%, cobalt 0.03%-0.09%, rare earth 0.15%-2.5%, yttrium 0.03%-0.5%, yttrium barium copper oxide 0.3%-0.8%, the total impurity content ≤0.3%, and the balance is aluminum.

2. The rare earth aluminum alloy high temperature resistant cable according to claim 1, characterized in that: The rare earth includes the following components in percentage by mass: praseodymium 0.02%-1.2%, lanthanum 0.03%-0.5%, cerium 0.03%-0.5%, and neodymium 0.03%-0.5%.

3. The rare earth aluminum alloy high temperature resistant cable according to claim 1, characterized in that: The invention comprises a rare earth aluminum alloy conductor, which is formed by twisting aluminum alloy monofilaments, a fire-resistant layer is arranged on the outside of the aluminum alloy conductor, an insulating layer is arranged on the outside of the fire-resistant layer, a glass fiber tape is wound on the outside of the insulating layer, at least one rare earth aluminum alloy conductor is arranged on the inside of the glass fiber tape, a high temperature resistant filler is arranged between the insulating layer and the glass fiber tape, an inner sheath layer is arranged on the outside of the glass fiber tape, an outer sheath layer is arranged on the outside of the inner sheath layer, and an armor layer is arranged between the inner sheath layer and the outer sheath layer.

4. The rare earth aluminum alloy high temperature resistant cable according to claim 1, characterized in that: The fire-resistant layer is a mica tape layer, the insulating layer is a polytrifluorochloroethylene layer, the high-temperature resistant filler is a ceramic silicone rubber, the armor layer is a galvanized steel tape layer, and the outer sheath layer is a low-smoke halogen-free layer.

5. A method for preparing a rare earth aluminum alloy high temperature resistant cable according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition; S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid; S3, smelting, adding weighed raw materials and low-oxygen hydrogenated dehydrogenated titanium powder into aluminum liquid for melting, adding grain refiner into the aluminum liquid, smelting, refining and degassing, melting evenly and then keeping warm to obtain rare earth aluminum alloy liquid; S4, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars; S5, rolling, rolling the rare earth aluminum alloy strip through a rolling mill to form a rare earth aluminum alloy rod with a diameter of Φ9.0 mm; S6, drawing, using a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical aluminum alloy monofilament, and twisting the aluminum alloy monofilament into a rare earth aluminum alloy conductor on a frame-type stranding machine using a special-shaped stranding die; S7, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing; S8, insulation, cabling, sheathing, after cooling, wrap a layer of mica tape on the outside of the rare earth aluminum alloy conductor to form a fire-resistant layer, and extrude the insulation layer with polytrifluorochloroethylene; fill the insulation layer with ceramic silicone rubber high-temperature resistant filler, and after filling, wrap it with glass fiber tape to form a cable and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with low-smoke halogen-free material to form a cable.

6. The method for preparing a rare earth aluminum alloy high temperature resistant cable according to claim 5, characterized in that: In the S2, the purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 750°C-800°C.

7. The method for preparing a rare earth aluminum alloy high temperature resistant cable according to claim 5, characterized in that: In the S3, the grain refiner is Al-5Ti-B refiner, and the mass percentage of grain refinement is 0.5%-1%.

8. The method for preparing a rare earth aluminum alloy high temperature resistant cable according to claim 5, characterized in that: In the S7, the annealing temperature is 300°C±10°C, and the annealing time is 6 hours to 9 hours.

9. The method for preparing a rare earth aluminum alloy high temperature resistant cable according to claim 5, characterized in that: The elongation of the prepared aluminum alloy monofilament is ≥35%, and the tensile strength is 135N / mm 2 -170N / mm 2 , 90° bending times more than 30 times, DC resistivity ≤0.0278Ω / m at 20℃, conductivity 62%-63%, bending radius 7D-12D, compared with copper cable, its rebound performance is reduced by 45%, compared with aluminum core cable, its creep resistance is increased by 350%, and its service life is not less than 45 years.

Citation Information

Patent Citations

  • Rare earth high-iron aluminum alloy fireproof cable and preparation method thereof

    CN111724942A

Cited By

  • Rare earth aluminum alloy monofilament as well as preparation method and application thereof

    CN120041712A

  • Rare earth aluminum alloy monofilaments, their preparation methods and applications

    CN120041712B