Neodymium-iron-boron permanent magnet with ultralow lanthanum and cerium impurities and preparation method of neodymium-iron-boron permanent magnet

By improving the smelting process of neodymium iron boron permanent magnets, using boron oxide to react with lanthanum cerium elements and removing scum, the problem of degradation of magnetic properties caused by lanthanum cerium elements is solved, and more stable high-temperature magnetic properties and low-cost production are achieved. Widely applied value.

CN118969427APending Publication Date: 2024-11-15ZHEJIANG INNUOVO MAGNETICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411161210.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the production of NdFeB permanent magnets, the presence of lanthanum and cerium elements leads to a decrease in magnetic properties, especially high-temperature magnetic properties, and improved processes are needed to reduce the content of lanthanum and cerium elements to improve magnetic properties.

Method used

By improving the smelting process, boron oxide (B2O3) is added to react with lanthanum cerium elements, solid scum is generated and removed, the alloy liquid temperature and stirring time are controlled, and the content of lanthanum cerium elements in the magnet is less than 10ppm and 100ppm, and secondary feeding is used Prepare low-lanthanum cerium impurity neodymium iron boron magnets by high-temperature sintering.

Benefits of technology

It effectively reduces the content of lanthanum cerium in the magnet, improves the high-temperature magnetic performance, is low in cost and easy to operate, and has great promotion and application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

According to the neodymium-iron-boron permanent magnet with the ultralow lanthanum and cerium impurities, boron oxide is added through secondary feeding in the smelting procedure, oxygen is introduced, lanthanum and cerium elements in the magnet are oxidized, and the lanthanum and cerium elements are used as scum for impurity removal, so that the content of the lanthanum and cerium elements in the magnet is reduced, the total La element content of the obtained magnet is not higher than 10 ppm, and the total Ce element content of the obtained magnet is not higher than 100 ppm; the content of the element O is not higher than 1000 ppm, the content of the element La in the grain boundary phase is not higher than 500 ppm, and the content of the element Ce in the grain boundary phase is not higher than 300 ppm. The lanthanum and cerium impurity content in the magnet is remarkably reduced through the simple method, and the high-temperature magnetic performance of the magnet is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of rare earth permanent magnetic materials and provides a neodymium iron boron permanent magnet with ultra-low lanthanum and cerium impurities and a preparation method thereof. Background Art

[0002] Neodymium iron boron magnets are known as the third generation of permanent magnet materials. They have excellent magnetic properties and are widely used in many fields such as motors, audio, and nuclear magnetic resonance.

[0003] The main rare earth elements used in the production of NdFeB permanent magnets are praseodymium and neodymium. 14 The B phase has a high saturation magnetization intensity, which is the main source of the high remanence of NdFeB magnets. In rare earth deposits, multiple rare earth elements usually coexist. Due to the rare earth smelting process and other reasons, the raw material commonly used to produce NdFeB permanent magnets is praseodymium-neodymium metal (Pr-Nd). The praseodymium-neodymium metal raw material usually contains a small amount of lanthanum and cerium. As recorded in the national standard GB / T 20892-2020 praseodymium-neodymium metal, the content of La is less than 0.05-0.1%, and the content of Ce is less than 0.05-0.1%. However, RE2Fe composed of lanthanum and cerium 14 The saturation magnetization, magnetocrystalline anisotropy field, and Curie temperature of the B phase are all lower than those of the RE2Fe phase of the NdPr composition. 14 B phase, which causes the magnetic properties of NdFeB magnets containing LaCe, especially the high-temperature magnetic properties, to decrease, which limits the use of the magnets under certain high-temperature working conditions.

[0004] In order to avoid the adverse effects of lanthanum and cerium on magnetic properties, it is necessary to improve the production process of NdFeB permanent magnets, reduce the lanthanum and cerium content in the magnets, and improve the high-temperature magnetic properties of NdFeB magnets. Summary of the invention

[0005] The purpose of the present invention is to provide a NdFeB permanent magnet with ultra-low lanthanum and cerium impurities and a preparation method thereof. The solution reduces the content of lanthanum and cerium elements in the magnet by improving the smelting process, so that the magnet can have relatively stable high-temperature magnetic properties.

[0006] The technical solution adopted by the present invention is:

[0007] A neodymium iron boron permanent magnet with low lanthanum and cerium impurities, the magnet comprising the following components in mass fractions:

[0008] R: 28wt%~34wt%,

[0009] R is a rare earth element, including one or more of Pr, Nd, Tb, Dy, Ho, and Gd;

[0010] B: 0.88wt%~1.05wt%,

[0011] Co: 0.5wt%~2wt%;

[0012] M: 0.1wt% to 3.5wt%, M is one or more elements selected from Al, Ti, Cu, Ga, Zr, and Nb;

[0013] The balance is iron and other unavoidable impurities;

[0014] The impurities contain La, Ce and O elements. In the magnet, the total La content is not higher than 10 ppm, the total Ce content is not higher than 100 ppm, and the O content is not higher than 1000 ppm.

[0015] Preferably, R contains at least one or two of Pr and Nd elements, and more preferably, R contains at least Pr and Nd;

[0016] Preferably, the magnet comprises a grain boundary phase, the La content in the grain boundary phase is not higher than 500 ppm, and the Ce content in the grain boundary phase is not higher than 300 ppm.

[0017] The NdFeB permanent magnet with low lanthanum and cerium impurities can be prepared by the following method:

[0018] (1) Sampling and component analysis of rare earth raw materials to calculate the mass fraction of La and Ce elements in the total amount of raw materials to be smelted La 、w Ce ;

[0019] (2) taking each raw material according to the composition ratio, vacuum melting until all the raw materials are melted, and then adding B2O3 into the crucible by secondary feeding;

[0020] (3) Control the alloy liquid temperature within the range of 1440-1490°C, and stir and refine for 5-15 minutes;

[0021] (4) removing scum, cooling to 1400-1440° C., casting, and obtaining flakes with low lanthanum and cerium impurities;

[0022] (5) The NdFeB magnets with low lanthanum and cerium impurities are obtained by hydrogen crushing, air flow grinding, orientation molding, isostatic pressing, high temperature sintering and aging treatment.

[0023] In the step (2), according to the mass m of La and Ce elements contained in the raw materials La 、m Ce Determine the amount of B2O3 added, the calculation formula is as follows:

[0024] The coefficient k is in the range of [0.8, 1.1].

[0025] The particle size of B2O3 powder is above 100 mesh, preferably 100-300 mesh.

[0026] k can be adjusted according to the reaction efficiency and the impurity removal conditions of the feeding test. Preferably, the range of k is 0.9-1.

[0027] The present invention also provides a method for preparing the NdFeB permanent magnet with low lanthanum and cerium impurities, the method comprising the following steps:

[0028] (1) Sampling and component analysis of rare earth raw materials to calculate the mass fraction of La and Ce elements in the total amount of raw materials to be smelted La 、w Ce ;

[0029] (2) taking each raw material according to the composition ratio, vacuum melting until all the raw materials are melted, and then adding B2O3 into the crucible by secondary feeding;

[0030] According to the La and Ce element mass m contained in the raw materials La 、m Ce Determine the amount of B2O3 added, the calculation formula is as follows:

[0031] The coefficient k is in the range of [0.8, 1.1];

[0032] (3) Control the alloy liquid temperature within the range of 1440-1490°C, and stir and refine for 5-15 minutes;

[0033] (4) removing scum, cooling to 1400-1440° C., casting, and obtaining flakes with low lanthanum and cerium impurities;

[0034] (5) The NdFeB magnets with low lanthanum and cerium impurities are obtained by hydrogen crushing, air flow grinding, orientation molding, isostatic pressing, high temperature sintering and aging treatment.

[0035] According to the Pauling electronegativity scale, the electronegativity of La, Ce, Pr, and Nd is 1.1, 1.12, 1.13, and 1.14, respectively. La and Ce are more active than Pr and Nd and are more easily oxidized. B2O3 has a low melting point of only about 450°C. In the present invention, B2O3 is added by secondary feeding during smelting, and B2O3 can be easily dispersed in the molten liquid to provide oxygen elements without excessive volatilization or introduction of other impurities.

[0036] The invention has the advantages of providing a preparation process of a NdFeB permanent magnet with ultra-low lanthanum and cerium impurities, adding boron oxide during the smelting process to react with lanthanum and cerium impurity elements in the molten metal to generate solid scum which is removed, thereby reducing the content of La and Ce elements in the magnet, having low cost and convenient operation, and the obtained magnet has more stable high-temperature magnetic properties and has great promotion and application value. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments. The embodiments described below are exemplary and are only used to better understand the present invention, and should not be construed as limiting the present invention.

[0038] Example 1

[0039] The total weight of the smelting raw materials is 600kg, and the contents of Pr, Nd, Fe, Co, Cu, Ga, Zr and B are 7.7wt%, 23.1wt%, 66.84wt%, 0.5wt%, 0.2wt%, 0.4wt%, 0.3wt% and 0.96wt% respectively. The raw materials of Pr and Nd are PrNd-75NdA with a purity of more than 99.98wt%, Zr comes from industrial ZrFe, B comes from industrial BFe alloy, and the balance of Fe is supplemented by pure iron. The remaining raw materials are pure metals, including metal Co with a purity of more than 99.99wt%, metal Cu with a purity of more than 99.99wt%, and metal Ga with a purity of more than 99.999wt%.

[0040] The raw materials of Pr and Nd are praseodymium-neodymium metal PrNd-75NdA. Composition analysis shows that the contents of La and Ce in the praseodymium-neodymium metal are 0.020wt% and 0.056wt% respectively.

[0041] It can be calculated that the mass fraction of La and Ce elements in the total amount of raw materials to be smelted is w La =61.6ppm, w Ce =172.48ppm. Substitute the data into the formula

[0042] Taking the coefficient k as 0.95, the mass of B2O3 required is calculated to be 41.6g. All raw materials are put into a vacuum melting furnace and heated. During the melting process, after observing that the solid in the crucible is completely melted, 41.6g of B2O3 powder with a particle size of 200 mesh is added to the crucible by secondary feeding. The temperature of the molten liquid is controlled within the range of 1450-1470℃, and after magnetic stirring and refining for 10 minutes, the scum is removed and the temperature is allowed to stand and cool down. When the temperature in the crucible is measured to be within the range of 1410-1430℃, the low lanthanum cerium impurity flakes are immediately cast. The flakes are subjected to hydrogen crushing, air flow grinding, orientation molding, isostatic pressing, high temperature sintering and aging treatment to obtain NdFeB magnets.

[0043] The composition of the NdFeB magnet was analyzed using an inductively coupled plasma emission spectrometer, and the contents of La, Ce, and O were found to be 7.48 ppm, 61.158 ppm, and 965 ppm, respectively.

[0044] The grain boundary phase composition in the NdFeB magnet was analyzed using a scanning electron microscope electron probe microanalysis, and the contents of La and Ce were found to be 0.03% and 0.028% respectively.

[0045] The magnetic properties were measured and the results are shown in Table 1 below:

[0046] Table 1

[0047]

[0048] Comparative Example 1

[0049] The formula and process are consistent with those in Example 1, and no additional B2O3 is added during smelting. The specific process is:

[0050] All raw materials are put into a vacuum melting furnace, heated to 1450-1470℃, magnetically stirred and refined for 3 minutes, and then left to cool down. When the temperature in the crucible is measured to be in the range of 1410-1430℃, the casting is immediately cast to obtain a fling sheet. The casting sheet is subjected to hydrogen crushing, air flow grinding, orientation molding, isostatic pressing, high temperature sintering and aging treatment to obtain a NdFeB magnet.

[0051] The composition of the NdFeB magnet was measured, and the contents of La, Ce, and O were 54.88ppm, 163.72ppm, and 782ppm, respectively.

[0052] The grain boundary phase composition of NdFeB magnets was analyzed by scanning electron microscope electron probe microanalysis, and the contents of La and Ce were found to be 0.07% and 0.041% respectively.

[0053] The magnetic properties were measured and the results are shown in Table 2 below:

[0054] Table 2

[0055]

[0056] It can be seen from Comparative Example 1 and Example 1 that the B2O3 added during smelting effectively consumes the lanthanum and cerium elements, thereby reducing the content of lanthanum and cerium elements in the magnet and improving the magnetic properties at high temperatures.

Claims

1. A NdFeB permanent magnet with ultra-low lanthanum and cerium impurities, Features The magnet comprises the following components in mass fractions: R: 28wt%~34wt%, R is a rare earth element, including R1 or R1 and R2, R1 is one or more of Pr, Nd, Tb, Dy, Ho, and Gd; B: 0.88wt%~1.05wt%, Co: 0.5wt%~2wt%; M: 0.1wt% to 3.5wt%, M is one or more elements selected from Al, Ti, Cu, Ga, Zr, and Nb; The balance is iron and other unavoidable impurities; The impurities contain La and Ce elements. In the magnet, the total La content is not higher than 10 ppm, and the total Ce content is not higher than 100 ppm.

2. The NdFeB permanent magnet with ultra-low lanthanum and cerium impurities as claimed in claim 1, wherein the content of O in the magnet is not higher than 1000 ppm.

3. The NdFeB permanent magnet with ultra-low lanthanum and cerium impurities as claimed in claim 1, Features The magnet comprises a grain boundary phase, the La content in the grain boundary phase is not higher than 500 ppm, and the Ce content in the grain boundary phase is not higher than 300 ppm.

4. The NdFeB permanent magnet with ultra-low lanthanum and cerium impurities as claimed in claim 1, Features R contains at least one or two of Pr and Nd elements.

5. The NdFeB permanent magnet with ultra-low lanthanum and cerium impurities as claimed in claim 1, Features The NdFeB permanent magnet with low lanthanum and cerium impurities is prepared by the following method: (1) Sampling and component analysis of rare earth raw materials to calculate the mass fraction of La and Ce elements in the total amount of raw materials to be smelted La 、w Ce ; (2) Take the raw materials according to the composition ratio, vacuum melt until all the raw materials are melted, and then add B into the crucible by secondary feeding. 2 O 3 ; According to the La and Ce element mass m contained in the raw materials La 、m Ce Determine B 2 O 3 The amount of addition is calculated as follows: The coefficient k is in the range of [0.8, 1.1]; (3) Control the alloy liquid temperature within the range of 1440-1490°C, and stir and refine for 5-15 minutes; (4) removing scum, cooling to 1400-1440° C., casting, and obtaining flakes with low lanthanum and cerium impurities; (5) The NdFeB magnets with low lanthanum and cerium impurities are obtained by hydrogen crushing, air flow grinding, orientation molding, isostatic pressing, high temperature sintering and aging treatment.

6. A method for preparing the ultra-low lanthanum-cerium impurity NdFeB permanent magnet according to any one of claims 1 to 5, Features The method comprises the following steps: (1) Sampling and component analysis of rare earth raw materials to calculate the mass fraction of La and Ce elements in the total amount of raw materials to be smelted La 、w Ce ; (2) Take the raw materials according to the composition ratio, vacuum melt until all the raw materials are melted, and then add B into the crucible by secondary feeding. 2 O 3 ; According to the La and Ce element mass m contained in the raw materials La 、m Ce Determine B 2 O 3 The amount of addition is calculated as follows: The coefficient k is in the range of 0.8 to 1.1; (3) Control the alloy liquid temperature within the range of 1440-1490°C, and stir and refine for 5-15 minutes; (4) removing scum, cooling to 1400-1440° C., casting, and obtaining flakes with low lanthanum and cerium impurities; (5) The NdFeB magnets with low lanthanum and cerium impurities are obtained by hydrogen crushing, air flow grinding, orientation molding, isostatic pressing, high temperature sintering and aging treatment.

7. The method according to claim 6, Features The B2O3 powder has a particle size of more than 100 meshes.

8. The method according to claim 6, wherein k is in the range of 0.9 to 1.