Mold for producing injection-molded magnet, injection-molded magnet and preparation method

By dynamically charging the injection molded magnet at the ejection path, using improved mold structure and magnetization device, the dimensional instability and magnetic performance differences of injection molded magnets in high temperature and high humidity environments are solved, and efficient and low-cost magnet production is achieved .

CN118969483APending Publication Date: 2024-11-15CHENGDU SILVER MAGNETIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185754.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing injection molded magnets are unstable in high temperature and high humidity environments, and have a risk of cracking. The magnetic properties vary greatly and are difficult to control, which affects the normal use of the motor.

Method used

Adopting an improved injection mold structure, by dynamically charging the injection molding magnet at the top-out path, the magnetization device forms a low magnetic field in the molding cavity, and the magnet is magnetized by the magnetization device when it is removed from the mold, and is provided by permanent magnet or electromagnetic magnetization device. High consistency magnetic field.

Benefits of technology

Effectively control the magnetic dispersion of injection molded magnets, reduce design and maintenance costs, improve production efficiency and cost-effectiveness, and take into account dimensional stability and magnetic performance consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969483A_ABST
    Figure CN118969483A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of permanent magnet production, and particularly relates to a mold for injection molding magnet production, an injection molding magnet and a preparation method. By designing the structure of the injection mold, a technical concept of performing dynamic magnetizing on an ejection path of the injection-molded magnet is provided, so that the dispersity of the magnetic performance of the injection-molded magnet is effectively controlled; and the magnetizing device is not subjected to pressure load and thermal load, so that the design and the implementation are easier, and the manufacturing and maintenance cost is lower. According to the design, the injection molding magnet melt can be fully oriented, meanwhile, the injection molding pressure and the injection molding temperature can be borne, the service life is economically feasible, and high-consistency magnetizing on an ejection path through a permanent magnet magnetizing device or an electromagnetic magnetizing device can be stably achieved. According to the technical scheme, the control cost, the size stability, the low magnetic energy density and the magnetic performance difference of the product can be considered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of permanent magnet production, and particularly relates to a mold for producing an injection-molded magnet, an injection-molded magnet and a preparation method. Background Art

[0002] Injection molded magnets are widely used in various motors and electronic products because they can be processed into complex shapes with high precision. Injection molded magnets are mainly bonded magnets produced by injection molding after thermoplastic binders and magnetic powders are mixed and granulated. In order to meet the magnet processing performance and mechanical strength, the binder must reach a certain content. Due to the low cost of PA6, the most commonly used thermoplastic binder in the prior art is nylon PA6, but nylon 6 is a plastic containing more hydrophilic amide groups, and its water absorption rate is significantly higher than that of PPS and even PA12. High temperature will accelerate the material to absorb water and expand, so the size changes greatly under high temperature and high humidity environment, the size is unstable, and there is even a risk of failure such as cracking. If used in a motor, there may be interference with other components, thereby affecting the normal use of the motor. Injection molded ferrite magnets with the following characteristics are difficult to produce: 1. Low magnetic energy density; 2. Small difference in magnetic properties between products; 3. High dimensional stability; 4. Relatively low production cost.

[0003] In order to make the injection molded magnet take into account the advantages of the above four aspects, the following methods have been tried:

[0004] a. Use nylon 6 + ferrite powder with low magnetic powder filling amount as raw material and use normal orientation field strength for production. However, this solution has low dimensional stability after wet heat due to the increase in the proportion of nylon 6 that absorbs water.

[0005] b. Use nylon 6 + ferrite powder with a high magnetic powder filling amount as raw material and adopt low field strength orientation method for production. However, the magnetic powder in the injection molded magnetic material under low orientation field strength is not fully oriented in this scheme, and the orientation state and the resulting magnet performance are greatly affected by the raw materials and injection molding process. The performance of the finished product fluctuates greatly, and it is difficult to effectively control the performance of the magnet, resulting in poor consistency of the motor.

[0006] c. Use nylon 12 or PPS + ferrite powder with a lower magnetic powder filling amount as raw material and use a stronger oriented magnetic field arranged near the mold cavity for production. However, this solution will significantly increase the production cost because the price of nylon 12 and PPS + ferrite powder is significantly higher than that of nylon 6 + ferrite powder. Summary of the invention

[0007] The purpose of the present invention is to provide a mold for producing an injection molded magnet, an injection molded magnet and a preparation method thereof in view of the technical defects in the prior art of low-performance injection molded magnets prepared using a relatively cheap PA6 matrix, large differences in magnetic properties between different batches of injection molded magnets and poor dimensional stability.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] A mold for preparing an injection-molded magnet, comprising:

[0010] A first module, a second module, an ejection assembly, and a magnetization assembly;

[0011] The first module is provided with a first cavity, a molding cavity and a magnetizing cavity which are connected and coaxially arranged in sequence, the first cavity and the molding cavity are both annular structures, and the magnetizing cavity is a cylindrical structure;

[0012] The ejector assembly is disposed in the first cavity, the cross section of the ejector assembly is smaller than the cross section of the first cavity, and the ejector assembly can move along the central axis of the first module; the ejector assembly is used to eject the injection magnet from the molding cavity;

[0013] The magnetization component is arranged around the periphery of the magnetization cavity;

[0014] The second module matches the magnetization cavity.

[0015] In the technical solution of the present invention, by improving the structure of the injection mold, a technical concept of dynamic magnetization in the ejection path of the injection molding magnet is proposed. The magnetic field generated by the magnetization device forms a magnetic field strength of <500Gs in the molding cavity; and a magnetic field area of ​​>2000Gs is formed on the surface of the magnetized area of ​​the path through which the injection molding magnet escapes from the mold, thereby magnetizing the magnet.

[0016] In the prior art, the magnetic properties of magnets are that the melt containing magnetic powder, under the action of the oriented magnetic field distributed in the mold cavity, deflects the magnetic moment direction of the magnetic powder to a direction close to the direction of the external magnetic field before the melt solidifies, thereby obtaining the external magnetic properties. In this process, many factors, including the difference in the oriented magnetic field, the slight change in temperature, the viscous flow of the melt, etc., will affect the magnetic properties of the final injection-molded magnet. In the scheme of the present invention, there is no magnetic field in the mold cavity that can significantly orient the magnetic powder in the injection-molded melt, and after the injection-molded magnet is completely solidified, it is magnetized by the magnetization device arranged on the ejection path, which has multiple positive effects including the following points:

[0017] a. The magnetic performance of injection molding magnets mainly depends on the performance level of magnetic particles during injection molding and the magnetization conditions provided by the magnetizing device on the ejection path, and has nothing to do with the various variable process parameters during the injection molding process, so that the dispersion of the magnetic properties of injection molding magnets can be effectively controlled.

[0018] b. The orientation device of the prior art is subject to high stress (e.g. 50MPa-100MPa) and high temperature (e.g. 270℃-330℃) in the mold cavity during injection molding, which makes it difficult to design and limits its service life. In the technical solution of the present invention, the magnetization device is not subject to pressure load and heat load, which makes it easier to design and implement, and the cost of manufacturing and maintenance is also lower.

[0019] c. Especially for magnets with narrow poles, specifically, the inner diameter ODm of the magnetizing device and the number of poles n formed by the magnetizing device have the following relationship: ODm / n≤2mm. Since the distance between the two adjacent poles is very close, the magnetic field strength decays very quickly with the distance from the wall of the orientation device. The design can fully orient the injection molding magnet melt and at the same time meet the injection molding pressure and injection molding temperature, and have an economically feasible life. By adopting the scheme of the present invention, magnetization with high consistency can be achieved more stably on the ejection path through a permanent magnet magnetizing device or an electromagnetic magnetizing device.

[0020] d. Compared with the process of first injection molding and then magnetizing by another device, the advantage of the present invention is that it uses one process to complete the common effects of the previous two processes and auxiliary processes such as transportation and packaging between the processes, which has significantly higher production efficiency and lower production costs.

[0021] As a more preferred technical solution, the second module includes a first channel and a second channel that are connected and coaxially arranged in sequence, the first channel is used to assemble with the magnetization cavity, the longitudinal section of the first channel is in the shape of a circular ring, and the area of ​​the circular ring gradually increases from the first channel to the central axis direction of the second channel. When the molten material is injected into the mold, it first passes through the second channel and then passes through the first channel to enter the molding cavity of the first module.

[0022] As a more preferred technical solution, the magnetization device is an electromagnetic type. The electromagnetic solution has a high magnetic field strength, which can make the magnetic properties of the magnet more consistent, but the magnetization timing needs to be controlled in a linked manner.

[0023] Specifically, the skeleton of the magnetization device is made of a material with an initial relative permeability > 50 and a saturation magnetization intensity > 1 T. The inner hole of the skeleton and the magnetization cavity can be separated by a low-permeability material with an initial relative permeability < 10 and a wall thickness t < ODm / n (ODm and n are the inner diameter of the magnetization device and the number of poles formed by the magnetization device, respectively), or not separated. There are an even number of wire grooves in the magnetization device skeleton, and one or more wires with an insulation resistance > 5 MΩ between the wires and the high-permeability material are arranged in each wire groove. When direct current is passed, if there are multiple wires arranged in each wire groove, then on a longitudinal section perpendicular to the inner hole axis, the angles formed by the current directions of the wires in all the same wire grooves < 3°, and the current direction of the wires arranged in the nearest adjacent wire groove > 177°.

[0024] As a more preferred technical solution, the magnetization device includes an even number of magnetic steel blocks, and a plurality of the magnetic steel blocks surround to form a Halbach array. Using a permanent magnet magnetization device can make the product production control simpler, without the positioning discharge control requirements of the electromagnetic magnetization scheme. Since the heat load received by the magnetic steel here is very small, a neodymium iron boron magnet with a higher remanence and relatively lower heat resistance can be used as the preferred solution for the magnetic steel magnet.

[0025] As a more preferred technical solution, the following relationship exists between the inner diameter ODm of the magnetization device and the number of poles n formed by the magnetization device: ODm / n ≤ 2 mm.

[0026] As a more preferred technical solution, the following relationship exists between the inner diameter ODm of the magnetization device and the number of poles n formed by the magnetization device: ODm / n ≤ 1 mm.

[0027] Since the pole width has a huge impact on the distribution gradient of the magnetic field, the solution described in the present invention has a more obvious technical comparison advantage when the pole width of the orientation device and the corresponding injection molded magnet is relatively narrow.

[0028] As a more preferred technical solution, the present invention provides an injection molded magnet prepared by the above injection molded magnet preparation mold. The injection molded magnet is composed of the following raw materials in parts by weight: 85% - 92% of permanent magnet magnetic powder, 7% - 13% of thermoplastic resin, and the balance is additives.

[0029] As a more preferred technical solution, the permanent magnet magnetic powder is a permanent ferrite magnetic powder, the thermoplastic resin is nylon 6, and the additives include at least one of a coupling agent, an antioxidant, a lubricant, and a plasticizer.

[0030] As a more preferred technical solution, after the injection molded magnet is placed in a damp and hot environment at 83°C - 87°C and a relative humidity of 80% - 90% for 100 h, the ratio of the corresponding outer dimension Lx of the injection molded magnet to the initial outer dimension Lx0 has the following relationship: 0 ≦ (Lx - Lx0) / Lx0 ≦ 0.8%

[0031] As a more preferred technical solution, the present invention provides an injection molded magnet molding method, which is carried out by preparing the injection molded magnet mold as described above, and specifically includes the following steps:

[0032] Step 1, spraying a coupling agent on one or more magnetic powders mixed in proportion, mixing and drying to obtain a first material;

[0033] Step 2, adding a binder and an antioxidant or a lubricant to the first material, stirring and mixing to form a second material, and extruding and granulating the second material at 200° C. to 280° C. to form pellets;

[0034] Step 3, using an injection molding machine and the above-mentioned injection mold, the pellets are melted at a temperature of 270° C. to 330° C. and a pressure of not less than 30 MPa, and then injected into the molding mold cavity in the first module through the first channel and the second channel for injection molding to form an injection molded intermediate;

[0035] Step 4: Push the injection molded intermediate out through an ejection assembly and magnetize it at the magnetization cavity to obtain an injection molded magnet product.

[0036] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0037] The technical solution of the present invention innovatively proposes a mold structure, which realizes the technical concept of dynamic magnetization in the ejection path of the injection molded magnet, so that the dispersion of the magnetic properties of the injection molded magnet is effectively controlled; the magnetization device is not subject to pressure load and heat load, is easier to design and implement, and has lower manufacturing and maintenance costs.

[0038] The design can fully orient the injection-molded magnet melt and at the same time can withstand the injection molding pressure and injection molding temperature and have an economically feasible life.

[0039] The technical solution of the present invention can take into account cost control, dimensional stability, low magnetic energy density and magnetic property differences of products. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 is a schematic structural diagram of a first module of the injection mold of the present invention;

[0041] Figure 2 It is a structural schematic diagram of the first module and the second module of the injection mold of the present invention;

[0042] Figure 3 It is a schematic structural diagram of the injection-molded magnet of the present invention after being ejected from the first module of the injection mold;

[0043] Figure 4 It is the AA plane section view;

[0044] Figure 5 It is the BB surface section view;

[0045] Figure 6 It is the CC plane section view;

[0046] Figure 7 It is an electromagnetic component;

[0047] icon:

[0048] 1- First module;

[0049] 11-first cavity; 12-molding cavity; 13-magnetization cavity;

[0050] 2- Second module;

[0051] 21-first channel; 22-second channel;

[0052] 3-magnetization component; 4-ejection component; 5-injection magnet; 6-low magnetic permeability material; 7-magnetization wire; 8-high magnetic permeability material. DETAILED DESCRIPTION

[0053] In order to more clearly describe the invention purpose, technical scheme and technical effect advantages in the specific implementation case of the present invention, the scheme in the specific embodiment will be described in detail in combination with the drawings of the specification of the present invention. The specific technical scheme involved in the following specific embodiments is only for a clear and complete description of the innovative technical scheme of the present invention. It is only a part of the specific implementation scheme that can be adopted by the present invention, not all embodiments, and should not be understood as a limitation on the innovative scheme of the present invention. Any scheme adopting the same inventive concept of the present invention should be included in the protection scope of the present invention.

[0054] Secondly, the description of the drawings in the specific embodiments of the present invention is only for the convenience of technical personnel to understand the solution of the present invention. The partial details in the drawings are for the convenience of clearly presenting the technical solution. It should not be considered that all technical features in the drawings must be included in the specific implementation cases, and the detailed features in the drawings should not be identified as additional limitations on the innovative technical solution of the present invention. The components in the various embodiments described and shown in the drawings can be combined and arranged according to different configurations, and these changes in combination and arrangement should be identified as part of the entire embodiment of the innovative solution of the present invention and included in the scope of protection of the present invention.

[0055] The present invention will be described in detail below in conjunction with the accompanying drawings.

[0056] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0057] Example 1

[0058] This embodiment provides a mold for preparing an injection molded magnet. Figure 1-Figure 6 As shown, specifically, the mold includes a first module, a second module, an ejection assembly and a magnetization assembly; the first module is provided with a first cavity, a molding cavity and a magnetization cavity that are connected and coaxially arranged in sequence, the first cavity and the molding cavity are both annular structures, and the magnetization cavity is a cylindrical structure;

[0059] The ejection assembly is arranged in the first cavity, the cross-section of the ejection assembly is smaller than the cross-section of the first cavity, and the ejection assembly can move along the central axis of the first module; the ejection assembly is used to eject the injection magnet from the molding cavity; the magnetization assembly is arranged around the periphery of the magnetization cavity; the second module matches the magnetization cavity.

[0060] In this embodiment, Figure 4-5 As shown, the inner diameter of the first cavity is represented by R1, the inner diameter of the molding die cavity is represented by R2, R1≤R2, and the range of R2 is 5mm~150mm.

[0061] As a more preferred technical solution, the second module includes a first channel and a second channel that are connected and coaxially arranged in sequence, the first channel is used to assemble with the magnetization cavity, the longitudinal section of the first channel is in the shape of a circular ring, and the area of ​​the circular ring gradually increases from the first channel to the central axis direction of the second channel. When the molten material is injected into the mold, it first passes through the second channel and then passes through the first channel to enter the molding cavity of the first module.

[0062] In the injection molding magnet preparation mold of the present invention, the magnetization component includes two forms. This embodiment specifically adopts the electromagnetic form. The structure of this form of magnetization component is as follows: Figure 7 As shown: 6 is a low magnetic permeability material, specifically an initial relative magnetic permeability <10, such as 304, HPM75, 7 is a magnetized wire, and 8 is a high magnetic permeability material, specifically a material with an initial relative magnetic permeability >50 and a saturation magnetization intensity >1T.

[0063] Example 2

[0064] This embodiment provides a mold for preparing an injection molded magnet, and its structure is basically the same as that of Embodiment 1, except that the magnetization component is a permanent magnetization device, i.e., a Halbach array. Figure 6As shown: the use of permanent magnet magnetization device can make product production control simpler, and does not require the control requirements of the positioning discharge of the electromagnetic magnetization scheme. Because the heat load on the magnetic steel here is very small, the neodymium iron boron magnet with higher remanence and relatively low heat resistance can be used as the preferred solution for the magnetic steel magnet.

[0065] In this embodiment, the inner diameter ODm of the magnetizing device and the number of poles n formed by the magnetizing device have the following relationship: ODm / n≤2mm.

[0066] Example 3

[0067] This embodiment provides a method for forming an injection molded magnet, which is specifically implemented by the mold of Embodiment 1, and includes the following steps:

[0068] Step 1: Drying the injection molded magnet granules to obtain a first material;

[0069] Step 2: using an injection molding machine to heat the injection molding magnet granules to 300° C., and injecting them into the mold cavity after melting;

[0070] Step 3 After the magnet is formed in the molding cavity, it is ejected into the magnetization cavity by the ejection mechanism;

[0071] Step 4: The magnet is magnetized in the magnetization cavity to obtain a finished injection molded magnet.

[0072] Injection molding magnet granules: Raw materials composed of nylon 6 with high magnetic powder filling amount + ferrite magnetic powder: GIM-FA2 granules of Chengdu Yinci Material Co., Ltd.

[0073] Example 4

[0074] In order to examine the dimensional stability of injection molded magnet products of different batches, this embodiment prepares the target injection molded magnet as follows. The injection molding method refers to the method of Example 2, and the injection mold refers to the structure of Example 1. This embodiment provides injection molded magnet samples #1-#6, which are prepared through 6 consecutive batches, and their product information is summarized in Table 1 below: The injection molded magnet has an outer diameter of Φ10.2mm, an inner diameter of Φ5.4mm, a height of 8.8mm, and an outer circle with 16 poles of radial magnetization, and its ODm / n=0.64mm≤1mm.

[0075] As shown in the performance summary data in Table 1, in Example 4, the injection molded magnets #1-#6 have stable dimensions, and the dimensional change rate is no higher than the specification value of 0.8%. In this embodiment, the peak value difference of the surface magnetism is no higher than 60Gs, and the surface magnetism angle deviation is controlled within 1°.

[0076] Example 5

[0077] This embodiment provides an injection molded magnet product #7, which is prepared by the mold of embodiment 2, and the injection molded magnet molding method is obtained by embodiment 3. The difference between it and embodiment 4 is that the magnetizing device in the mold is a permanent magnetizing device.

[0078] In this embodiment, the pellets of GIM-FA2 brand of Chengdu Yinci Material Co., Ltd. are used. The injection molded magnet has an outer diameter of Φ10.2mm, an inner diameter of Φ5.4mm, a height of 8.8mm, and an outer circle radial 16-pole magnetization, and its ODm / n=0.64mm≤1mm. Its product information is summarized in Table 1 below. It can be seen from the data statistics in Table 1 that, whether it is electromagnetic or permanent magnetization, the injection molded magnets obtained by the technical solution of the present invention have better performance in all aspects than the prior art.

[0079] Example 6

[0080] This embodiment provides an injection molded magnet product, the injection molding method is as in Example 3, the injection mold and the magnetization device are as in Example 1, and the pellets of GIM-FA2 brand from Chengdu Yinci Material Co., Ltd. are used. The injection molded magnet has an outer diameter of Φ22mm, an inner diameter of Φ10mm, a height of 5mm, and is magnetized with 16 poles in the outer radial direction, and its ODm / n=1.39mm≤2mm.

[0081] Example 7

[0082] This embodiment provides an injection molded magnet product, the injection molding method is as in the embodiment 3, the injection mold and the magnetization device are as in the embodiment 1, and the pellets of GIM-FA2 brand from Chengdu Yinci Material Co., Ltd. are used. The injection molded magnet has an outer diameter of Φ18mm, an inner diameter of Φ12mm, a height of 12.8mm, and an outer radial 24-pole magnetization, and its ODm / n=0.75mm≤1mm.

[0083] Example 8

[0084] This embodiment provides an injection-molded magnet product, the injection molding method is as in the embodiment 3, the injection mold and the magnetization device are as in the embodiment 1, and the pellets of GIM-FA2 brand from Chengdu Yinci Material Co., Ltd. are used. The injection-molded magnet has an outer diameter of Φ32.8 mm, an inner diameter of Φ23.5 mm, a height of 30 mm, and an outer radial 24-pole magnetization, and its ODm / n=1.37 mm≤2 mm.

[0085] Comparative Example 1

[0086] This comparative example provides an injection molded magnet product, which uses a raw material composed of nylon 6 + ferrite powder with a relatively low magnetic powder filling amount: Chengdu Silver Magnetic Material GIM-FA1.3 grade granules. During the injection molding process, the normal orientation field strength of the permanent magnet magnetization device arranged near the mold cavity is used for orientation. The injection molded magnet has an outer diameter of Φ10.2mm, an inner diameter of Φ5.4mm, a height of 8.8mm, and an outer circle with 16 radial poles. Its ODm / n=0.64mm≤1mm. Its product information is summarized in Table 1 below.

[0087] Comparative Example 2

[0088] This comparative example provides an injection molded magnet product, which uses a raw material composed of nylon 6 + ferrite powder with a high magnetic powder filling amount: Chengdu Silver Magnetic Material GIM-FA2 grade granules. And during the injection molding process, the orientation field of a low-field strength permanent magnet magnetization device arranged near the mold cavity is used for orientation. The injection molded magnet has an outer diameter of Φ10.2mm, an inner diameter of Φ5.4mm, a height of 8.8mm, and an outer circle radially magnetized with 16 poles, and its ODm / n=0.64mm≤1mm. This embodiment provides injection molded magnet samples #1-#6, and the samples #1-#6 are prepared through 6 consecutive batches. The product information is summarized in Table 1 below.

[0089] Comparative Example 3

[0090] This comparative example provides an injection molded magnet product, which uses a raw material composed of nylon 12 + ferrite powder with a relatively low magnetic powder filling amount: the GIM-FB1.6 grade granules of Chengdu Silver Magnetic Material are oriented by the orientation field of the normal field strength permanent magnet magnetization device arranged near the mold cavity. The injection molded magnet has an outer diameter of Φ10.2mm, an inner diameter of Φ5.4mm, a height of 8.8mm, and an outer circle radial 16-pole magnetization, and its ODm / n=0.64mm≤1mm. Its product information is summarized in Table 1 below.

[0091] Comparative Example 4

[0092] This comparative example provides an injection molded magnet product, which uses a raw material composed of PPS + ferrite powder with a relatively low magnetic powder filling amount: GIM-FC1.5 grade granules of Chengdu Silver Magnetic Materials, and is oriented using an orientation field of a normal field strength permanent magnet magnetization device arranged near the mold cavity. The injection molded magnet has an outer diameter of Φ10.2mm, an inner diameter of Φ5.4mm, a height of 8.8mm, and an outer circle radial 16-pole magnetization, and its ODm / n=0.64mm≤1mm. Its product information is summarized in Table 1 below.

[0093] Comparative Example 5

[0094] This comparative example provides an injection molded magnet product, the injection molding method is as in Example 3, the injection mold and the magnetization device are as in Example 2, and the pellets of GIM-FA2 brand from Chengdu Yinci Material Co., Ltd. are used. The injection molded magnet has an outer diameter of Φ29.85mm, an inner diameter of Φ17mm, a height of 13mm, and an outer radial 4-pole magnetization, and its ODm / n=7.46mm≥2mm. Its product information is summarized in Table 2 below.

[0095] Comparative Example 6

[0096] This comparative example provides an injection molded magnet product, which uses a raw material composed of nylon 6 + ferrite powder with a high magnetic powder filling amount: Chengdu Silver Magnetic Material GIM-FA2 grade granules. During the injection molding process, the orientation field of the permanent magnet magnetization device with normal field strength placed near the mold cavity is used for orientation. The injection molded magnet has an outer diameter of Φ29.85mm, an inner diameter of Φ17mm, a height of 13mm, and an outer circle radial 4-pole magnetization, and its ODm / n=7.46mm≥2mm. Its product information is summarized in Table 2 below.

[0097] Embodiment 4 and embodiment 5 are the improved solutions of the present invention, and comparative examples 1-4 are the existing solutions, among which comparative example 1 has a high dimensional change rate after the wet heat test and cannot meet the requirements, comparative example 2 has large differences in product performance and poor consistency, and comparative examples 3 and 4 have very high costs.

[0098] The product dimensions and performance are shown in the table below, where the damp heat test is to measure the rate of change of the outer diameter after being placed in a damp heat environment of 83℃~87℃ and 80%~90% relative humidity for 100 hours.

[0099] Table 1 is a comparison summary of existing technical solutions and improved technical solutions for Φ10.2*Φ5.4*8.8 outer circle radial 16-pole magnetization

[0100]

[0101] Table 2 is a summary of product information of Examples 6-8 and Comparative Examples 5-6

[0102]

[0103] Examples 6, 7, and 8 are the technical solutions of the present application, and comparative examples 5-6 are ODm / n>2mm. In this case, the surface magnetic peak value extreme difference and surface magnetic angle deviation of the technical solution of the present invention and the technical solution of the prior art are not much different.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A mold for producing injection molded magnets, characterized in that: include: A first module, a second module, an ejection assembly, and a magnetization assembly; The first module is provided with a first cavity, a molding cavity and a magnetizing cavity which are connected and coaxially arranged in sequence, the first cavity and the molding cavity are both annular structures, and the magnetizing cavity is a cylindrical structure; The ejector assembly is disposed in the first cavity, the cross section of the ejector assembly is smaller than the cross section of the first cavity, and the ejector assembly can move along the central axis of the first module; the ejector assembly is used to eject the injection magnet from the molding cavity; The magnetization component is arranged around the periphery of the magnetization cavity; The second module matches the magnetization cavity.

2. The mold for producing injection molded magnets according to claim 1, characterized in that: The second module includes a first channel and a second channel that are connected and coaxially arranged in sequence. The first channel is used to be assembled with the magnetization cavity. The longitudinal section of the first channel is in the shape of a circular ring. The area of ​​the circular ring gradually increases from the first channel to the central axis direction of the second channel.

3. The mold for producing injection molded magnets according to claim 2, characterized in that: The magnetizing means is in the form of an electromagnetic magnetizing device.

4. The mold for producing injection molded magnets according to claim 2, characterized in that: The magnetization device includes an even number of magnetic steel blocks, and a plurality of the magnetic steel blocks surround to form a Halbach array.

5. The mold for producing injection molded magnets according to claim 3, characterized in that: The inner diameter ODm of the magnetizing device and the number of poles n formed by the magnetizing device have the following relationship: ODm / n≤2mm.

6. The mold for producing injection molded magnets according to claim 3, characterized in that: The inner diameter ODm of the magnetizing device and the number of poles n formed by the magnetizing device have the following relationship: ODm / n≤1mm.

7. An injection molded magnet made by the mold for producing an injection molded magnet according to any one of claims 1 to 6, characterized in that: The injection-molded magnet is composed of the following raw materials in parts by weight: 85%-92% of permanent magnetic powder, 7%-13% of thermoplastic resin, and the remainder of additives.

8. The injection molded magnet according to claim 7, characterized in that: The permanent magnetic powder is permanent ferrite magnetic powder, the thermoplastic resin is nylon 6, and the additives include at least one of a coupling agent, an antioxidant, a lubricant, and a plasticizer.

9. The injection molded magnet according to claim 7, characterized in that: After the injection molded magnet is placed in a hot and humid environment with a temperature range of 83° C. to 87° C. and a relative humidity range of 80% to 90% for not less than 100 hours, the ratio of the outer dimension Lx corresponding to the injection molded magnet to the initial outer dimension Lx0 has the following relationship: 0≦(Lx-Lx0) / Lx0≦0.8%.

10. A method for forming an injection molded magnet, characterized in that: The mold according to any one of claims 1 to 6 is prepared, and the preparation method comprises the following steps: Step 1, spraying a coupling agent on one or more magnetic powders mixed in proportion, mixing and drying to obtain a first material; Step 2, adding a binder and an antioxidant or a lubricant to the first material, stirring and mixing to form a second material, and extruding and granulating the second material at 200° C. to 280° C. to form pellets; Step 3, using an injection molding machine and the injection mold according to any one of claims 1 to 6, the pellets are melted at a temperature of 270° C. to 330° C. and a pressure of not less than 30 MPa, and then injected into the molding mold cavity in the first module through the first channel and the second channel for injection molding to form an injection molded intermediate; Step 4: Push the injection molded intermediate out through an ejection assembly and magnetize it at the magnetization cavity to obtain an injection molded magnet product.