Packaging substrate and manufacturing method thereof
Through exposure dose adjustment and plasma etching technology, the production of embedded metal wiring layers in semiconductor packaging substrates is simplified, solving the problems of complex processes and high costs, and achieving efficient and environmentally friendly metal wiring layers, improving accuracy and reliability sex.
Patent Information
- Application Number
- CN202411066124.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the production process of buried metal wiring layers in the semiconductor field is complex and costly, especially when the line width/line distance is less than 5/5um, it is difficult to realize traditional wet process, resulting in low production efficiency and increased cost.
An exposure dose adjustment mechanism is used to expose the resist layer at different exposure doses, forming the first and second grooves, and the production of the metal wiring layer is achieved through plasma etching, simplifying the process and reducing costs.
The graphic production of the metal wiring layer is achieved at one time, shortening the manufacturing process, reducing equipment, materials, labor, space and time costs, improving the quality and dimensional accuracy of the metal wiring layer, and avoiding wear through the buried wiring structure. , improves reliability and yield.
Smart Images

Figure CN118969729A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a packaging substrate and a manufacturing method thereof. Background Art
[0002] With the development of Moore's Law, the integration of ultra-large-scale integrated circuit chips has reached a scale of up to billions of devices, with multi-layer and high-density fine lines, and its wiring is quite complicated. Since metal copper cannot form volatile byproducts, in the semiconductor field, the etching of metal copper cannot be achieved by traditional dry etching. At the same time, in order to solve the resistance and parasitic capacitance problems caused by high-density metal connections, the metal interconnection process based on the dual Damascene process is gradually being applied to the field of micro-semiconductor integrated circuit device manufacturing. For example, the most commonly used through-hole method at present requires first making a barrier layer-dielectric layer-barrier layer-dielectric layer-hard mask structure on the surface of the wafer, and then through two times of resist coating-exposure-development and dry etching of the dielectric layer, through holes and grooves are made on the dielectric layer respectively, and finally the production is completed by electroplating copper and chemical mechanical grinding. Although this method can well solve the problem of dry etching of metal copper, it has many processing steps and a complicated process flow, which not only affects production efficiency, but also greatly increases production costs.
[0003] In the field of advanced packaging, although the production of metal copper wires is still based on the mature SAP (Semi-additive Process) / ET (Embedded Trace) process, in order to continue Moore's Law in another way, advanced packaging has also begun to develop towards a multi-layer high-density packaging structure with finer lines. Usually, when the line width / line spacing (L / S) is less than 5 / 5um, it is difficult for metal lines to be produced through traditional wet processes. For this reason, the industry usually uses the Full Via First manufacturing process of the Damascus process to solve this problem, but this process requires two photolithography processes when forming through holes and line grooves, so the product preparation process is long and the cost is high. There is also a method of grayscale mask lithography to achieve 3D graphics production of line grooves and through holes at one time, but the preparation of the mask is very difficult, the cost is very high, and the processing flexibility is also limited.
[0004] In view of this, there is an urgent need for a method for manufacturing a packaging substrate that can realize the manufacturing of an embedded metal wiring layer at one time and can simplify the process and reduce the manufacturing cost. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a packaging substrate and a method for manufacturing the same, so as to solve the problems of complex manufacturing process and high manufacturing cost of the buried metal wiring layer in the prior art.
[0006] To achieve the above object and other related objects, the present invention provides a method for manufacturing a packaging substrate, comprising the following steps:
[0007] Providing a substrate, and forming a resist layer on at least one functional surface of the substrate;
[0008] Providing an exposure dose adjustment mechanism, using the exposure dose adjustment mechanism to expose the first area and the second area of the resist layer to a first preset exposure dose and a second preset exposure dose respectively, wherein the first preset exposure dose is less than the second preset exposure dose, and at least one of the first areas is located outside the second area;
[0009] Based on the first area and the second area after exposure, a first groove and a second groove are formed in the resist layer respectively, wherein the first groove penetrates the resist layer, and the second groove opens from the surface of the resist layer away from the substrate and the bottom is spaced a preset distance from the surface of the substrate;
[0010] A metal wiring layer is formed to fill the first groove and the second groove, and the resist layer and the metal wiring layer constitute a wiring structure.
[0011] Optionally, the resist layer comprises positive photoresist.
[0012] Optionally, the exposure dose adjustment mechanism includes a grating light valve.
[0013] Optionally, the method of forming the first groove includes plasma etching; and the method of forming the second groove includes plasma etching.
[0014] Optionally, when the first groove and the second groove are formed by plasma etching, the method further includes a step of regulating the current field, temperature field and air flow field in the plasma chamber.
[0015] Optionally, the first groove includes a first portion and a second portion that are connected, the first portion opens from the top of the resist layer and the bottom of the first portion is connected to the top of the second portion, and the bottom of the second portion exposes the functional surface of the substrate.
[0016] Optionally, a transverse cross-sectional dimension of the first portion is greater than a transverse cross-sectional dimension of the second portion.
[0017] Optionally, forming the metal wiring layer includes the following steps: forming a pre-plated metal layer covering the surface of the resist layer, the bottom and side walls of the first groove, and the bottom and side walls of the second groove, forming a metal connection layer covering the surface of the pre-plated metal layer and filling the first groove and the second groove, and removing the pre-plated metal layer and the metal connection layer located on the surface of the resist layer to obtain the metal wiring layer filling the first groove and the second groove.
[0018] Optionally, a plurality of wiring structures stacked in sequence are formed on the functional surface of the substrate, and in two adjacent wiring structures, the metal wiring layer in the wiring structure away from the substrate is electrically connected to the metal wiring layer in the wiring structure close to the substrate.
[0019] The present invention further provides a packaging substrate, wherein the packaging substrate is manufactured by using any of the above-mentioned methods for manufacturing the packaging substrate.
[0020] As described above, the packaging substrate and the manufacturing method thereof of the present invention have the following beneficial effects: by using the exposure dose adjustment mechanism to perform exposure of the first preset exposure dose and the second preset exposure dose in the first area and the second area inside the resist layer respectively, and setting the first preset exposure dose to be less than the second preset exposure dose, at least one of the first areas is located outside the second area, and then plasma etching is used to form the first groove and the second groove inside the exposed resist layer, so that the pattern production of the metal wiring layer is completed at one time, which greatly shortens the manufacturing process of the packaging substrate, thereby comprehensively reducing the equipment, material, labor, space and time costs, and because in In the production process of the packaging substrate, no potentially harmful chemicals need to be used, and the production method is more green and environmentally friendly. The exposure dose is controlled by the exposure dose adjustment mechanism, which reduces the errors generated in the production process and improves the quality and dimensional accuracy of the metal wiring layer. In addition, the production method of the packaging substrate of the present invention is different from the metal wiring layer protruding outward produced by the traditional subtractive method, semi-additive method and additive method. The metal wiring layer is buried inside the resist layer, which avoids wear and tear during subsequent processes and transportation, greatly improving the reliability and yield of the packaging substrate, and also solves the problem that the redundant pre-plated metal layer and the metal connection layer in the fine circuit are difficult to remove by dry etching at one time. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram showing the manufacturing process of the packaging substrate of the present invention.
[0022] Figure 2 It is a schematic diagram of the structure after forming the resist layer of the present invention.
[0023] Figure 3 It is a schematic diagram showing the structure of the present invention after the resist layer is exposed.
[0024] Figure 4 It is a schematic diagram of the structure after forming a first groove and a second groove of the present invention.
[0025] Figure 5 It is a schematic diagram of the structure after forming the pre-plated metal layer of the present invention.
[0026] Figure 6 It is a schematic diagram of the structure after forming the metal connection layer of the present invention.
[0027] Figure 7 It is a schematic diagram of the structure after forming the metal wiring layer of the present invention.
[0028] Figure 8 It is a schematic diagram of the structure after forming a multi-layer wiring structure of the present invention.
[0029] Component number description
[0030] 1 substrate
[0031] 2. Resist layer
[0032] 3. District 1
[0033] 4. District 2
[0034] 5 First groove
[0035] 51 Part 1
[0036] 52 Part 2
[0037] 6 Second groove
[0038] 7 Metal wiring layer
[0039] 71 Pre-plated metal layer
[0040] 72 Metal connection layer
[0041] 8 Wiring structure DETAILED DESCRIPTION
[0042] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0043] See also Figures 1 to 8. It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings in this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no substantial technical significance. Any modification of the structure, change in the proportional relationship, or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effects and purposes that can be achieved by the present invention. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in this specification are only for the convenience of description, and are not used to limit the scope of the implementation of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the implementation of the present invention without substantially changing the technical content.
[0044] Embodiment 1
[0045] Figure 1 FIG. 1 is a schematic diagram of a manufacturing process of a packaging substrate. This embodiment provides a method for manufacturing a packaging substrate, comprising the following steps:
[0046] S1: providing a substrate, and forming a resist layer on at least a functional surface of the substrate;
[0047] S2: providing an exposure dose adjustment mechanism, using the exposure dose adjustment mechanism to perform exposure of a first preset exposure dose and a second preset exposure dose on a first area and a second area of the resist layer respectively, wherein the first preset exposure dose is less than the second preset exposure dose, and at least one first area is located outside the second area;
[0048] S3: Based on the exposed first area and the second area, a first groove and a second groove are formed in the resist layer respectively, wherein the first groove penetrates the resist layer, and the second groove opens from the surface of the resist layer away from the substrate and the bottom is spaced a preset distance from the surface of the substrate;
[0049] S4: forming a metal wiring layer filling the first groove and the second groove, the resist layer and the metal wiring layer constitute a wiring structure.
[0050] For details, please refer to Figure 2 , perform step S1, provide a substrate 1, and form a resist layer 2 on at least a functional surface of the substrate 1.
[0051] Specifically, the functional surface of the substrate 1 refers to a surface for forming the subsequent wiring structure 8 . In the present embodiment, the functional surface refers to at least one of the upper and lower surfaces of the substrate 1 .
[0052] Specifically, the substrate 1 includes a core plate (not shown) stacked in sequence, a dissociation layer (not shown) coated on the upper surface of the core plate, and a conductive metal layer (not shown) located on the upper surface of the dissociation layer.
[0053] Specifically, the material of the core board includes one of glass, ceramics and organic materials or other suitable materials.
[0054] Specifically, the material of the dissociation layer includes one of epoxy resin, phenolic resin, polyester resin or other suitable materials.
[0055] Specifically, the material of the conductive metal layer includes copper or other suitable materials.
[0056] Specifically, Figure 2 , which is a schematic diagram of the structure after the resist layer 2 is formed. The method of forming the resist layer 2 includes coating, vacuum lamination or other suitable methods.
[0057] Specifically, when the resist layer 2 is formed by coating, the coating methods used include spin coating and slit coating.
[0058] As an example, the resist layer 2 includes positive photoresist or other suitable types of photoresist. In this embodiment, positive photoresist is used as the resist layer 2. Since it is easily soluble in organic solvents such as ether, ester, ketone, etc. and has a high resolution, the resist layer 2 can be used to obtain submicron-level graphics in the subsequent processing process.
[0059] Specifically, the thickness of the resist layer 2 is in the range of 30 to 40 μm.
[0060] For details, please refer to Figure 3 , execute step S2, provide an exposure dose adjustment mechanism (not shown), and use the exposure dose adjustment mechanism to expose the first area 3 and the second area 4 inside the resist layer 2 to a first preset exposure dose and a second preset exposure dose respectively, wherein the first preset exposure dose is less than the second preset exposure dose, and at least one first area 3 is located outside the second area 4.
[0061] As an example, the exposure dose adjustment mechanism (not shown) includes a grating light valve or other suitable adjustment mechanism.
[0062] Specifically, Figure 3 As shown, it is a schematic diagram of the structure after the resist layer 2 is exposed. The exposure of the resist layer 2 includes the following steps: providing an exposure dose adjustment mechanism including a projection objective lens, generating a mask pattern in real time based on the exposure dose adjustment mechanism to obtain an exposure dose distribution with three-dimensional morphological features, using a projection objective lens to proportionally reduce the mask pattern and project it into the resist layer 2, and exposing the first area 3 and the second area 4 in the resist layer 2 to a first preset exposure dose and a second preset exposure dose, wherein the first preset exposure dose is less than the second preset exposure dose, and at least one first area 3 is located outside the second area 4.
[0063] Specifically, the grating light valve is a device unit composed of an even number of parallel strip structures made on a silicon substrate, which is staggered with movable strips and fixed strips, with two support points at both ends of the strips, and suspended in a very thin air layer (thickness <1um) in the middle, and the surface of the strip structure is aluminum-plated to improve reflectivity and conductivity, and the lower surface of the strip structure serves as a common electrode. It should be noted that the size of the strip structure can be adjusted as needed, and the strip structure is made of silicon nitride material, which can provide higher tension and durability.
[0064] Specifically, an aluminum layer is plated on the surface of the strip structure, and the reflectivity and conductivity can be improved by plating aluminum on the surface of the strip structure.
[0065] Specifically, during the operation of the grating light valve, a certain voltage is applied to one half of the movable strips, and the strips can be moved up and down under the action of the electrostatic field. When no pressure is applied, the strips are in a taut state, the entire unit surface is flat, and is in a completely reflective state; when a voltage is applied between the movable strips and the substrate, multiple alternating strips can move downward, making the surface a phase grating. At this time, the grating light valve device is in a diffraction state, and a phase difference is generated between the light waves reflected by the fixed strips and the movable strips. The reflection or diffraction angle and intensity of the laser are controlled by controlling the bias voltage of different grating light valve units, and grayscale exposure of different exposure doses in different areas is achieved on the resist layer 2 on the substrate 1 through the projection objective.
[0066] Specifically, when the resist layer 2 is exposed, the laser is irradiated onto a one-dimensional grating light valve plane array through a lens. The exposure system controls the voltage of different grating light valve units according to the input graphic data, and the movable bar is displaced to different degrees according to the input voltage, thereby controlling the proportion of light reflection or diffraction and modulating the reflection or diffraction angle of the light path. Each grating light valve unit can independently modulate the incident light, so each pixel can be independently controlled during exposure, thereby achieving the purpose of controlling the exposure dose of different areas of the graphic and realizing grayscale exposure. Due to the different material properties and process parameters of different resist layers 2, generally speaking, the relationship between exposure depth and exposure dose does not change linearly, but generally changes according to the trend of a logarithmic function, which can be summarized as follows:
[0067] 0<h(x,y)<H,E th <E(x,y)<E cl , where the parameter γ represents the relative curvature and is a constant, E th represents the critical exposure dose (i.e., the minimum exposure dose that triggers the photochemical reaction of the dielectric layer), E clrepresents the exposure dose required to completely remove the dielectric layer H, and E(x, y) represents the exposure dose required to achieve the exposure depth h(x, y). The above formula can be used to obtain: From this formula, the exposure dose E(x, y) required for any height h(x, y) can be calculated, thereby obtaining an exposure dose model corresponding to the design structure. Finally, according to this model, it is ensured that the exposure depth achieved by using the first preset exposure dose and the second preset exposure dose can meet the required shape and depth of the first groove 5 and the second groove 6.
[0068] For details, please refer to Figure 4 , execute step S3, based on the exposed first area 3 and the second area 4, form a first groove 5 and a second groove 6 in the resist layer 2 respectively, the first groove 5 penetrates the resist layer 2, and the second groove 6 opens from the surface of the resist layer 2 away from the substrate 1 and the bottom is spaced a preset distance from the surface of the substrate 1.
[0069] As an example, Figure 4 As shown, it is a schematic diagram of the structure after forming the first groove 5 and the second groove 6. The method of forming the first groove 5 includes plasma etching or other methods; the method of forming the second groove 6 includes plasma etching or other methods.
[0070] Specifically, forming the first groove 5 and the second groove 6 includes the following steps: providing a plasma device, fixing the exposed resist layer 2 and the substrate 1 in a plasma chamber by a specific clamp, and then adjusting the three-dimensional direction of the carrier of the substrate 1 by the carrier clamp in the plasma chamber to ensure that the range of the warpage of the substrate 1 is within ±7mm, starting the plasma device, applying radio frequency voltage to the plasma source gas through the electrodes at both ends, and the gas in the area is excited by the high-frequency alternating electric field formed between the electrodes to form plasma, and then the plasma enters the plasma chamber from the movable plasma channel under the action of bias, and begins to selectively bombard the first area 3 and the second area 4 of the resist layer 2 after exposure with ions, and the volatiles of the reaction substances in the bombarded and reacted first area 3 and the second area 4 after exposure are extracted by the vacuum system, and this process is continued until all the reaction substances in the first area 3 and the second area 4 are removed, and then the first groove 5 and the second groove 6 can be formed in the resist layer 2. It should be noted that the independently arranged first region 3 after exposure is etched by plasma to form the second groove 6 , and the second region 4 and the first region 3 located outside the second region 4 are etched by plasma to form the first groove 5 .
[0071] Specifically, the type of plasma etching includes at least one of inductively coupled plasma (ICP), capacitively coupled plasma (CCP), and surface microwave plasma (SWP).
[0072] Specifically, the plasma source gas used for plasma etching to form the first groove 5 and the second groove 6 includes inert gas, corrosive gas, and oxidizing gas. Among them, the inert gas can be He, Ne, Ar, Kr, Xe, the corrosive gas can be Cl2, CO2, HCl, HF, etc., and the oxidizing gas can be O2 and CF series gas, etc.
[0073] It should be noted that if the materials of the reaction substances after exposure of the first area 3 and the second area 4 are different from those of the resist layer 2, the plasma source gas ratio can be adjusted according to the actual situation to improve the selection ratio, so as to ensure that the reaction substances in the first area 3 and the second area 4 will not cause excessive damage to the surfaces of the remaining structures when the reaction substances in the first area 3 and the second area 4 are removed. In addition, in addition to the reaction substances in the first area 3 and the second area 4, other inclusions or oxides on the surfaces of the first area 3 and the second area 4 can be removed by plasma bombardment in a purely physical manner, leaking out the first area 3 and the second area 4 that really need to be removed, accelerating the chemical reaction, and then continuously removing the volatilized gases of the reaction substances by vacuuming, and by continuously repeating the process of plasma reacting with the surfaces of the first area 3 and the second area 4 and the continuous volatilization of the reaction products, the reaction substances in the first area 3 and the second area 4 are finally removed very accurately in a unique way combining physical reaction and chemical reaction.
[0074] As an example, when the first groove 5 and the second groove 6 are formed by plasma etching, the step of regulating the current field, temperature field and air flow field in the plasma chamber is also included.
[0075] Specifically, by controlling the current field, temperature field and gas flow field in the plasma chamber, the uniformity of the plasma acting on the resist layer 2 and a good removal rate can be controlled.
[0076] Specifically, an electrode is disposed on the plasma chamber, and the electrode is located below the substrate 1 and coincides with a projection of the substrate in a vertical direction, and a negative bias generator is disposed below the electrode.
[0077] Specifically, by arranging an electrode on the plasma chamber, and arranging the electrode below the substrate and coinciding with the projection of the substrate in the vertical direction, when the plasma comes out of the plasma forming chamber, the plasma can have a directionality vertical or nearly vertical to the substrate 1, and can vertically bombard the first area 3 and the second area 4; and by arranging a negative bias generator below the electrode, a pulse current several times the intensity of the direct current is instantly generated, so that a very high density plasma is instantly generated near the substrate 1, ensuring that the reaction substances in the first area 3 and the second area 4 are fully removed, and it can also be ensured that the side walls of the first area 3 and the second area 4 will not be etched while removing the reaction substances, so that the subsequent first groove 5 and the second groove 6 can have a better morphology. In addition, the electrode is arranged outside the cavity, which can reduce the pollution in the plasma cavity during the reaction process.
[0078] Specifically, the temperature field in the plasma cavity is regulated by adjusting the radio frequency alternating current of the plasma device and connecting the carrier and the plasma cavity to a cooling circulation system. The cooling circulation system can take away the heat of the substrate 1 and the plasma cavity in time during the processing to ensure that the plasma cavity and the substrate 1 are in a suitable reaction temperature range, wherein the cooling medium can be a liquid or a gas. By regulating the temperature field in the plasma cavity, it is possible to avoid an increase in the ion incidence rate and energy due to an increase in the single etching amount, a longer etching time, and an increase in the temperature in the substrate 1 and the plasma cavity, thereby causing excessive etching, causing certain damage to the surface of the resist layer 2 or the substrate 1 and generating stress, and ultimately leading to poor etching.
[0079] Specifically, the regulation of the gas flow field is mainly achieved by controlling the processing efficiency and distribution of the plasma. Under the action of the induced electric field, the plasma enters the plasma chamber from the plasma channel. During the processing, the plasma channel can move at a uniform speed along the long side of the substrate 1 to ensure that the plasma can act evenly on the resist layer 2; at the same time, there are vacuum systems on both sides of the plasma chamber, and the vacuum degree can be adjusted according to the incident direction and position of the plasma, so as to better control the distribution of the incident ions, and the reaction generated gas can be discharged in time, thereby improving the efficiency of the plasma in removing the reaction substances.
[0080] As an example, the first groove 5 includes a first portion 51 and a second portion 52 that are connected. The first portion 51 opens from the top of the resist layer and the bottom is connected to the top of the second portion 52 . The bottom of the second portion 52 exposes the functional surface of the substrate 1 .
[0081] Specifically, the distance between the bottom of the first part 51 and the opening of the first groove 5 is the same as the thickness of the first zone 3, the distance between the bottom of the second part 52 and the opening of the first groove 5 is the same as the thickness of the second zone 4; the distance between the bottom of the second groove 6 and the opening of the second groove 6 is the same as the thickness of the first zone 3.
[0082] Specifically, the distance between the bottom of the second groove 6 and the surface of the substrate 1 is in the range of 5 to 8 μm.
[0083] Specifically, the size of the transverse cross section of the second portion 52 is in the range of 15 to 30 μm; and the distance between two adjacent first grooves 5 is in the range of 50 to 70 μm.
[0084] As an example, the transverse cross-sectional dimension of the first portion 51 is greater than the transverse cross-sectional dimension of the second portion 52. It should be noted that the transverse cross-sectional dimension here refers to the distance between the inner walls of the first portion 51 and the second portion 52 in the horizontal direction.
[0085] Specifically, under the condition that the performance of the packaging substrate is met, the shape and size of the first groove 5 formed can also be selected according to actual conditions; the shape and size of the second groove 6 formed can also be selected according to actual conditions.
[0086] Specifically, an exposure dose adjustment mechanism is used to expose the first area 3 and the second area 4 inside the resist layer 2 with a first preset exposure dose and a second preset exposure dose respectively, and the first preset exposure dose is set to be less than the second preset exposure dose, at least one first area 3 is located outside the second area 4, and plasma etching is then used to form a first groove 5 and a second groove 6 inside the exposed resist layer 2, thereby achieving a one-time completion of the pattern production of the metal wiring layer 7, greatly shortening the manufacturing process of the packaging substrate, and thereby comprehensively reducing the equipment, material, labor, space and time costs. In addition, since no potentially harmful chemicals need to be used in the production process of the packaging substrate, the production method is more green and environmentally friendly, and the exposure dose is controlled by the exposure dose adjustment mechanism, thereby reducing the errors generated in the production process and improving the quality and dimensional accuracy of the subsequently formed metal wiring layer 7.
[0087] For details, please refer to Figure 5-Figure 7 , perform step S4 to form a metal wiring layer 7 filling the first groove 5 and the second groove 6, and the resist layer 2 and the metal wiring layer 7 constitute a wiring structure 8.
[0088] Specifically, Figure 5-Figure 7 As shown, they are respectively a schematic diagram of the structure after forming a pre-plated metal layer 71, a schematic diagram of the structure after forming a metal connection layer 72, and a schematic diagram of the structure after forming a metal wiring layer 7. The formation of the metal wiring layer 7 includes the following steps: forming a pre-plated metal layer 71 covering the surface of the resist layer 2, the bottom and side walls of the first groove 5, and the bottom and side walls of the second groove 6, forming a metal connection layer 72 covering the surface of the pre-plated metal layer 71 and filling the first groove 5 and the second groove 6, and removing the pre-plated metal layer 71 and the metal connection layer 72 located on the surface of the resist layer 2 to obtain a metal wiring layer 7 filling the first groove 5 and the second groove 6.
[0089] Specifically, the method for forming the pre-plated metal layer 71 includes chemical plating, physical vapor deposition or other suitable methods. In this embodiment, the method for forming the pre-plated metal layer 71 is physical vapor deposition, because the thickness of the pre-plated metal layer 71 formed by physical vapor deposition has good controllability and repeatability, a wide range of applications, and good bonding with the resist layer 2 and the substrate 1.
[0090] Specifically, the material of the pre-plated metal layer 71 includes at least one of titanium and copper or other suitable metal materials. In this embodiment, by first forming a titanium layer, since the metal layer of the titanium layer has high electrical conductivity and adhesion, and is soft in texture, it is not easy to generate stress during the manufacturing process, and the subsequently formed metal connection layer 72 can be firmly fixed on the insulating layer 2 and the substrate 1, and then a copper layer with a thickness greater than the titanium layer is deposited on this basis to obtain the pre-plated metal layer 71.
[0091] Specifically, the thickness of the pre-plated metal layer 71 is in the range of 300-500 nm.
[0092] Specifically, the material of the metal connection layer 72 includes copper or other suitable conductive materials.
[0093] Specifically, the method for forming the metal connection layer 72 includes high-speed electroplating or other suitable methods. In this embodiment, the metal connection layer 72 is made by high-speed electroplating, which has higher electroplating efficiency and mass transfer, and can produce a metal connection layer 72 with higher quality and better uniformity.
[0094] Specifically, the high-speed electroplating method for producing the metal connection layer 72 includes the following steps: sequentially performing high-pressure water washing and high-pressure acid washing on the surface of the pre-plated metal layer 71, and electroplating, water washing and drying on the surface of the pre-plated metal layer 71 to obtain the metal connection layer 72, wherein the current density used in the high-speed electroplating can be 3 to 10 ASD.
[0095] Specifically, under the condition that the performance of the package substrate is met, the size of the metal connection layer 72 can be selected according to the actual situation, and is not limited here. In this embodiment, the thickness and line width ratio of the metal connection layer 72 is preferably 1:1, the thickness deviation of the metal connection layer 72 is <5%, and the thickness range is 5-10μm.
[0096] Specifically, the method of removing the pre-plated metal layer 71 and the metal connection layer 72 located on the surface of the resist layer 2 includes chemical mechanical polishing or other suitable methods.
[0097] Specifically, the use of chemical mechanical polishing to remove the pre-plated metal layer 71 and the metal connection layer 72 located on the surface of the anti-etching layer 2 includes the following steps: providing a chemical mechanical polishing device, placing the substrate 1 formed with the pre-plated metal layer 71 and the metal connection layer 72 on the chemical mechanical polishing device, and adding polishing liquid to the contact surface between the metal connection layer 72 and the chemical mechanical polishing device, and then grinding the pre-plated metal layer 71 and the metal connection layer 72, and monitoring the thickness of the pre-plated metal layer 71 and the metal connection layer 72 during the grinding process, repeating the process multiple times until the excess pre-plated metal layer 71 and the metal connection layer 72 located on the surface of the anti-etching layer 2 are completely removed, and ensuring that the surface of the anti-etching layer 2 is level without bumps or grooves.
[0098] As an example, Figure 8 , which is a schematic diagram of a structure after forming a multi-layer wiring structure 8, a multi-layer wiring structure 8 is formed on the functional surface of the substrate 1, and in two adjacent wiring structures 8, the metal wiring layer 7 in the wiring structure 8 far from the substrate 1 is electrically connected to the metal wiring layer 7 in the wiring structure 8 close to the substrate 1. It should be noted that the number of layers of the wiring structure 8 formed can be selected according to actual conditions.
[0099] Specifically, the metal wiring layer 7 is configured to be buried in the anti-etching layer 2, which is not easy to wear during subsequent processes and transportation, greatly improving the reliability and yield of the packaging substrate, and also solving the problem that the excess pre-plated metal layer 71 and metal connection layer 72 in the fine circuit are difficult to remove by dry etching at one time.
[0100] The method for manufacturing the packaging substrate of the present embodiment uses an exposure dose adjustment mechanism to perform exposure with a first preset exposure dose and a second preset exposure dose on the first area 3 and the second area 4 inside the resist layer 2, respectively, and sets the first preset exposure dose to be less than the second preset exposure dose, at least one first area 3 is located outside the second area 4, and then plasma etching is used to form a first groove 5 and a second groove 6 inside the exposed resist layer 2, thereby achieving one-time completion of the pattern production of the metal wiring layer 7, greatly shortening the manufacturing process of the packaging substrate, thereby comprehensively reducing the equipment, material, labor, space and time costs, and because no need is required in the manufacturing process of the packaging substrate By using chemicals that may cause harm, the production method is more green and environmentally friendly, and the exposure dose is controlled by an exposure dose adjustment mechanism, which reduces the errors generated in the production process and improves the quality and dimensional accuracy of the metal wiring layer 7; in addition, the production method of the packaging substrate of this embodiment is different from the outwardly protruding metal wiring layer 7 produced by the traditional subtractive method, semi-additive method and additive method. The metal wiring layer 7 is configured to be embedded, which avoids wear and tear during subsequent processes and transportation, greatly improves the reliability and yield of the packaging substrate, and also solves the problem that the excess pre-plated metal layer 71 and the metal connection layer 72 in the fine circuit are difficult to remove by dry etching at one time.
[0101] Embodiment 2
[0102] The present embodiment provides a packaging substrate, which is manufactured by the packaging substrate manufacturing method described in the first embodiment, and includes: a substrate 1, a first groove 5, a second groove 6 and at least one wiring structure 8, wherein the wiring structure 8 includes a resist layer 2 and a metal wiring layer 7, the first groove 5 penetrates the resist layer 2, the second groove 6 opens from the resist layer 2 away from the surface of the substrate 1 and the bottom is spaced a preset distance from the surface of the substrate 1, and the metal wiring layer 7 fills the first groove 5 and the second groove 6.
[0103] Specifically, the metal wiring layer 7 includes a stacked pre-plated metal layer 71 and a metal connection layer 72 .
[0104] Specifically, the metal wiring layer 7 is located inside the resist layer 2, that is, the metal wiring layer 7 is embedded, which avoids wear and tear during subsequent processes and transportation, and greatly improves the reliability and yield of the substrate.
[0105] The metal wiring layer 7 of the packaging substrate of the present embodiment is arranged to be embedded, which is not easily worn out during the subsequent manufacturing process and transportation, thus greatly improving the reliability and yield rate of the substrate.
[0106] In summary, the packaging substrate and the manufacturing method thereof of the present invention respectively perform exposure of the first preset exposure dose and the second preset exposure dose in the first area and the second area inside the resist layer by using an exposure dose adjustment mechanism, and set the first preset exposure dose to be less than the second preset exposure dose, at least one first area is located outside the second area, and then plasma etching is used to form the first groove and the second groove inside the exposed resist layer, thereby achieving one-time completion of the pattern production of the metal wiring layer, greatly shortening the manufacturing process of the packaging substrate, and thus comprehensively reducing the equipment, material, labor, space and time costs, and because no need is required in the manufacturing process of the packaging substrate The use of chemicals that may cause harm makes the production method more environmentally friendly, and the exposure dose is controlled by an exposure dose adjustment mechanism, which reduces the errors generated in the production process and improves the quality and dimensional accuracy of the metal wiring layer. In addition, the production method of the packaging substrate of this embodiment is different from the metal wiring layer protruding outward produced by the traditional subtractive method, semi-additive method and additive method. The metal wiring layer is buried inside the resist layer, which avoids wear and tear during subsequent processes and transportation, greatly improving the reliability and yield of the packaging substrate, and also solves the problem that the redundant pre-plated metal layer and metal connection layer in the fine circuit are difficult to remove by dry etching at one time. Therefore, the present invention effectively overcomes the various shortcomings of the prior art and has a high industrial utilization value.
[0107] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for manufacturing a packaging substrate, characterized in that: The following steps are involved: Providing a substrate, and forming a resist layer on at least one functional surface of the substrate; Providing an exposure dose adjustment mechanism, using the exposure dose adjustment mechanism to expose the first area and the second area of the resist layer to a first preset exposure dose and a second preset exposure dose respectively, wherein the first preset exposure dose is less than the second preset exposure dose, and at least one of the first areas is located outside the second area; Based on the first area and the second area after exposure, a first groove and a second groove are formed in the resist layer respectively, wherein the first groove penetrates the resist layer, and the second groove opens from the surface of the resist layer away from the substrate and the bottom is spaced a preset distance from the surface of the substrate; A metal wiring layer is formed to fill the first groove and the second groove, and the resist layer and the metal wiring layer constitute a wiring structure.
2. The method for manufacturing a packaging substrate according to claim 1, characterized in that: The resist layer includes positive photoresist.
3. The method for manufacturing a packaging substrate according to claim 1, characterized in that: The exposure dose adjustment mechanism includes a grating light valve.
4. The method for manufacturing a packaging substrate according to claim 1, wherein: The method of forming the first groove includes plasma etching; the method of forming the second groove includes plasma etching.
5. The method for manufacturing a packaging substrate according to claim 4, characterized in that: When the first groove and the second groove are formed by plasma etching, the method further includes a step of regulating the current field, temperature field and air flow field in the plasma chamber.
6. The method for manufacturing a packaging substrate according to claim 1, wherein: The first groove includes a first portion and a second portion that are connected. The first portion opens from the top of the resist layer and the bottom is connected to the top of the second portion. The bottom of the second portion exposes the functional surface of the substrate.
7. The method for manufacturing a packaging substrate according to claim 6, wherein: The transverse cross-sectional dimension of the first portion is greater than the transverse cross-sectional dimension of the second portion.
8. The method for manufacturing a packaging substrate according to claim 1, characterized in that: Forming the metal wiring layer includes the following steps: forming a pre-plated metal layer covering the surface of the resist layer, the bottom and side walls of the first groove, and the bottom and side walls of the second groove, forming a metal connection layer covering the surface of the pre-plated metal layer and filling the first groove and the second groove, and removing the pre-plated metal layer and the metal connection layer located on the surface of the resist layer to obtain the metal wiring layer filling the first groove and the second groove.
9. The method for manufacturing a packaging substrate according to claim 1, wherein: A plurality of wiring structures stacked in sequence are formed on the functional surface of the substrate, and in two adjacent wiring structures, the metal wiring layer in the wiring structure far from the substrate is electrically connected to the metal wiring layer in the wiring structure close to the substrate.
10. A packaging substrate, characterized in that: The packaging substrate is manufactured by using the packaging substrate manufacturing method according to any one of claims 1 to 9.