Method for preparing selective emitter based on low-temperature boron diffusion method and preparation method of crystalline silicon cell
Through low-temperature boron expansion method and laser film opening technology, the high manufacturing cost and degradation of battery performance caused by high temperature oxidation in SE technology are solved, and the selective emitter is prepared at low temperatures, reducing costs and improving battery performance.
Patent Information
- Application Number
- CN202411149357.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
AI Technical Summary
The existing SE technology laser direct doping method requires high temperature oxidation, resulting in high manufacturing costs, damage to the life of the matrix silicon wafer and degradation of battery performance, and the contact advantage of selective boron junctions cannot be achieved.
The low-temperature boron diffusion method is used to match the laser film. By depositing the BSG layer and the inkjet barrier layer on the front of the silicon wafer, the laser film and the low-temperature boron diffusion treatment are used to form a selective emitter, reducing manufacturing costs and protecting the life of the matrix.
The selective emitter is prepared at low temperature, reducing manufacturing costs, improving battery performance, avoiding damage to battery performance by high-temperature oxidation, and achieving concentration differences in light and heavy doping regions through different deposition amounts, improving contact resistance.
Smart Images

Figure CN118969866A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a method for preparing a selective emitter based on a low-temperature boron diffusion method, and a method for preparing a crystalline silicon cell. Background Art
[0002] In order to increase the proportion of photovoltaic power generation, cost reduction and efficiency improvement are the two main lines of photovoltaic manufacturing. At present, crystalline silicon solar cells still occupy the main market of photovoltaic cells. Regardless of the latest TOPCon technology or the current mainstream PERC cell technology, balancing the contact resistance of the emitter area, emitter recombination and metal recombination are the keys to improving efficiency. SE technology (selective emitter) is the current mainstream choice. This technology mainly forms a selective PN junction on the surface of the battery, that is, a heavy doping diffusion that can meet the contact resistance and metal recombination is used for the metal contact area, and a light doping diffusion with low emission and recombination is used for the remaining area to achieve the goal of simultaneously reducing the contact resistance, emitter recombination and metal recombination.
[0003] At present, the common SE technology in the industry is mainly laser direct doping: a preparation method that uses high-temperature boron diffusion (maximum temperature > 1030°C) and laser doping. The disadvantages of the existing SE technology laser direct doping scheme are: in order to meet the light doping passivation and post-alkali etching process matching, it is necessary to use an oxygen heat process greater than 1030°C, which leads to additional manufacturing costs; high-temperature oxidation is particularly serious for the life of the substrate silicon wafer and the front reflectivity, which will affect the Uoc and Isc performance of the battery; the heavy doping concentration cannot be increased, and the contact advantage of the selective boron junction cannot be reflected; laser pre-doping with a boron-rich layer to cool the tube will cause lattice damage in the lightly doped area and cause the battery performance to decline. It can be seen that the existing SE technology laser direct doping process is relatively complex, the manufacturing cost is high, and it has a certain degree of adverse effects on battery performance. Summary of the invention
[0004] In order to solve the above technical problems, a method for preparing a selective emitter based on low-temperature boron diffusion and a method for preparing a crystalline silicon cell are provided. The present invention adopts low-temperature boron diffusion (maximum temperature 900-1000°C) matched with laser film opening, which can realize the preparation of a selective emitter at low temperature, reduce the manufacturing cost, and the all-low-temperature process ensures the minority carrier lifetime of the substrate and improves the battery performance.
[0005] In order to achieve the above objectives, the present invention is implemented by the following technical solutions: The method for preparing a selective emitter based on a low temperature boron diffusion method comprises the following steps: S1, taking a double-sided textured silicon wafer, and depositing a BSG layer on the textured surface on the front side of the silicon wafer; S2, inkjet a barrier layer solution on the surface of the BSG layer, and form a barrier layer after drying; S3, performing laser film opening treatment on the barrier layer; S4. The samples after film opening are subjected to boron diffusion treatment. Since there is still a barrier layer in the unopened area, while the barrier layer and part of BSG in the opened area have been removed, after the boron diffusion treatment, the unopened area is lightly doped to form a lightly doped area due to the presence of the barrier layer, while the opened area is heavily doped to form a heavily doped area due to the absence of the barrier layer, thereby obtaining a silicon wafer containing a selective emitter.
[0006] Further, the barrier layer solution includes one or more substances selected from silicate, silanol, silicon nitride sol, sodium aluminate, and ammonium sulfate; silicate such as methyl silicate, ethyl silicate, propyl silicate, butyl silicate, etc.; silanol such as triphenylsilanol, triethylsilanol, triisopropylsilanol, tetramethylammoniumsilanol, tert-butyldimethylsilanol, etc.; After inkjetting the barrier layer solution, it is dried at 80-200° C. to constant weight. The barrier layer solution increases in weight by 1-10 mg after drying. The increased weight is adjusted by the mass concentration of the barrier layer solution. The increased weight reflects the thickness of the formed barrier layer.
[0007] Furthermore, a tubular device is used to deposit a BSG layer on the front side of the silicon wafer, and the deposition parameters are as follows: at a temperature of 600-900° C., a mixed gas of a boron source and oxygen is introduced for deposition for 200-600 seconds, and the volume ratio of the boron source to oxygen is 1:2-1:5.
[0008] Furthermore, the laser film opening process reaches the BSG layer, and retaining a partial thickness of the BSG layer can achieve no damage to the film opening area; the laser film opening process uses a 532nm pulsed laser for film opening, the film opening power is 10~30W, the spot size is 70~150μm, and the distance between two adjacent film opening areas is determined according to the graphic design requirements.
[0009] Furthermore, the boron expansion treatment is carried out in a low-pressure boron expansion tube, with the temperature set to 900~1000°C, the pressure set to 100~300mbar, the mixed gas of the boron source (such as BCl3, BBr3, etc.), the volume ratio of the boron source and oxygen is 1:2~1:5, the deposition time is 200~600s, and the advancement time is 1000~5000s.
[0010] Furthermore, the silicon wafer is an N-type single crystal silicon wafer, the thickness of the silicon wafer is 160-200 μm, and the resistivity is 0.3-2.1 Ω·cm; The velvet surface is a pyramid structure velvet surface, and the velvet surface height is 1-5 μm; The thickness of the BSG layer is 60-100 nm; The thickness of the barrier layer retained in the lightly doped region is 20-70 nm; The square resistance of the lightly doped region is 200-800Ω / sq, and the square resistance of the heavily doped region is 50-200Ω / sq.
[0011] Another aspect of the present invention provides a method for preparing a crystalline silicon cell, comprising the following steps: (1) Providing a silicon wafer comprising a selective emitter produced by the above-mentioned production method; (2) After removing the BSG layer on the back of the silicon wafer and performing alkali polishing, a tunnel oxide layer and an intrinsic amorphous silicon layer are sequentially formed on the back; (3) Then the phosphorus diffusion treatment completes the crystallization treatment at the same time, and a PSG layer is obtained on the surface; (4) After removing the front and edge plating and surface oxide layer, perform surface passivation treatment; (5) The electrodes are made by double-sided metallization process and then sintered to form crystalline silicon cells.
[0012] Furthermore, the process conditions for performing phosphorus diffusion treatment and completing crystallization treatment at the same time are: in a mixed gas of phosphorus source gas and oxygen, diffusion is performed at 700-900° C. for 800-4000 s, so that high-temperature crystallization and phosphorus diffusion can be completed simultaneously; The surface passivation treatment is: first use ALD to deposit aluminum oxide layers on both sides, and then use PECVD to prepare passivation anti-reflection film layers on both sides. The passivation anti-reflection film layers are selected from a single layer or any combination of multiple layers of silicon nitride film, silicon oxynitride film, and silicon oxide film.
[0013] Furthermore, the alkali polishing makes the back reflectivity greater than 40%; the thickness of the tunneling oxide layer is 1~2nm, the thickness of the intrinsic amorphous silicon deposition layer is 50~150nm; the thickness of the aluminum oxide layer is 3~10nm, the thickness of the front passivation anti-reflection film layer is 75~80nm, and the thickness of the back passivation anti-reflection film layer is 70~100nm; the back silver electrode is produced by the back metallization process, and the front aluminum electrode is produced by the front metallization process.
[0014] Beneficial technical effects: The present invention adopts a low-temperature boron diffusion matching laser film opening method to realize the preparation of the selective emitter. Specifically, after a BSG layer is deposited on the front velvet surface, a barrier layer is formed thereon. The barrier layer that blocks the diffusion of boron is used as compensation for the insufficient thickness of BSG in the low-temperature process. After the laser film opening, the difference in the deposition amount between the lightly doped area and the heavily doped area is realized through the barrier layer, so that the preparation of the selective emitter can be realized at a relatively low temperature. On the one hand, the method of the present invention greatly reduces the manufacturing cost, and the all-low-temperature process ensures the minority carrier lifetime of the matrix and improves the battery performance; at the same time, since the difference in concentration of light and heavy doping areas is achieved by the difference in deposition amount, the obtained selective emitter meets the demand for improving contact resistance and can improve battery performance. The first step of the BSG layer deposition is achieved under the condition of 600-800°C. During the process, B2O3 is generated as a boron source, which will not form doping, nor will it produce a boron-rich layer that is unfavorable to the battery. Cooling the outlet tube will not cause additional problems such as reduced battery performance; in addition, the demand for lasers in the present invention is not limited. Compared with the current direct doping technology that requires the use of specific lasers, the present invention can adjust the material absorption wavelength of the barrier layer for different lasers to achieve corresponding laser matching; The barrier layer in the present invention can completely block the subsequent boron diffusion to the lightly doped area, and can avoid the adverse effect on the uniformity of the square resistance of the lightly doped area; the present invention does not need to adopt the reverse etching process, and the method of adopting the barrier layer can better maintain the morphology and light trapping effect of the lightly doped area, while ensuring that the stability of the square resistance of the lightly doped area can be controlled in a more industrialized manner; this patent adopts inkjet of the barrier layer solution to realize the preparation of the barrier layer, which can more flexibly control the thickness of the barrier layer, without considering how to achieve a balance between the thickness of the oxide layer and the laser damage problem by laser oxidation in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The present invention is a process flow chart of the method for preparing a selective emitter based on the low-temperature boron diffusion method. DETAILED DESCRIPTION
[0016] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0017] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0018] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods. Example 1
[0019] Method for preparing selective emitter based on low temperature boron diffusion method, the process flow refers to Figure 1 , including the following steps: S1, select N-type single crystal silicon wafer with resistivity of 1.0~1.5Ω·cm, minority carrier lifetime>2.5ms, thickness of 170µm, and size of 210mm×210mm; The damaged layer on the surface of the silicon wafer is removed in a mixed solution of KOH and H2O2, and then double-sided texturing is performed in the KOH solution to form a pyramid velvet surface with a height of 3µm. After the texture surface is completed, a BSG layer is deposited on the front side of the silicon wafer using a tubular device. The deposition parameters are as follows: at a temperature of 650-900° C., a boron source and oxygen gas are introduced for deposition for 300-500 seconds. The volume ratio of the boron source to oxygen is 1:3-1:4. A low-concentration BSG layer with a thickness of 80-90 nm is obtained on the texture surface on the front side of the silicon wafer. S2. Inkjet ethyl silicate solution as a barrier layer solution on the surface of the front BSG layer. The ethyl silicate solution includes ethyl silicate and a volatile solvent (such as ethanol, water, or other solvents that can evaporate quickly at the subsequent temperature). Dry at 100-150°C to constant weight (according to the properties of the solvent, the relevant drying time to constant weight is obtained through optimization experiments. In this case, ethanol and water are used in a volume ratio of 3:7, and the drying time is about 60-80s) to form a barrier layer. After drying, the weight increases by 1.2-2.0mg; S3, performing laser film opening treatment on the barrier layer, wherein the laser film opening parameters are: using 532nm pulsed laser for film opening, film opening power of 15-20W, and spot size of 90-100μm; S4. Place the opened sample in a low-pressure boron expansion tube for boron expansion treatment. The boron expansion treatment parameters are as follows: temperature set at 950~980℃, pressure set at 160~200mbar, boron source (such as BCl3, BBr3, etc.) and oxygen, source-oxygen ratio 1:3~1:4, deposition time 400~600s, advancement time 3000~4000s. After the boron expansion treatment, a lightly doped area and a heavily doped area are formed. The square resistance of the lightly doped area is 400~600Ω / sq, and the square resistance of the heavily doped area is 120~150Ω / sq, and a silicon wafer containing a selective emitter is obtained. Example 2
[0020] Method for preparing selective emitter based on low temperature boron diffusion method, the process flow refers to Figure 1 , including the following steps: S1, select N-type single crystal silicon wafer with resistivity of 0.3~0.9Ω·cm, minority carrier lifetime>2.5ms, thickness of 170µm, and size of 210mm×210mm; The damaged layer on the surface of the silicon wafer is removed in a mixed solution of KOH and H2O2, and then double-sided texturing is performed in the KOH solution to form a pyramid velvet surface with a height of 1.8~2.2µm. After the texture surface is completed, a BSG layer is deposited on the front side of the silicon wafer using a tubular device. The deposition parameters are as follows: at a temperature of 600°C to 700°C, a boron source and oxygen gas are introduced for deposition for 200 to 400 seconds, and the source-oxygen ratio is 1:2 to 1:3, and a BSG layer with a thickness of 60 to 80 nm is obtained on the texture surface on the front side of the silicon wafer. S2. Inkjet ethyl silicate solution as a barrier layer solution on the surface of the front BSG layer. The ethyl silicate solution includes ethyl silicate and a volatile solvent (such as ethanol, water, or other solvents that can evaporate quickly at the subsequent temperature). Dry at 80-110°C to constant weight (according to the properties of the solvent, the relevant drying time to constant weight is obtained through optimization experiments. In this case, ethanol and water are used in a volume ratio of 2:8, and the drying time is about 100-200s) to form a barrier layer. After drying, the weight increases by 2.0-3.0mg; S3, performing laser film opening treatment on the barrier layer, wherein the laser film opening parameters are: using 532nm pulsed laser for film opening, film opening power of 12-18W, and spot size of 70-80μm; S4. Place the opened sample in a low-pressure boron expansion tube for boron expansion treatment. The boron expansion treatment parameters are as follows: temperature set at 900~950℃, pressure set at 120~160mbar, boron source (such as BCl3, BBr3, etc.) and oxygen, source-oxygen ratio 1:2~1:3.5, deposition time 200~450s, advancement time 2000~3000s. After the boron expansion treatment, a lightly doped area and a heavily doped area are formed. The square resistance of the lightly doped area is 500~800Ω / sq, and the square resistance of the heavily doped area is 150~200Ω / sq, and a silicon wafer containing a selective emitter is obtained. Example 3
[0021] Method for preparing selective emitter based on low temperature boron diffusion method, the process flow refers to Figure 1 , including the following steps: S1, select N-type single crystal silicon wafer with resistivity of 1.5~2.0Ω·cm, minority carrier lifetime>2.5 ms, thickness of 170µm, and size of 210mm×210mm; The damaged layer on the surface of the silicon wafer is removed in a mixed solution of KOH and H2O2, and then double-sided texturing is performed in the KOH solution to form a pyramid velvet surface with a height of 1.8~2.2µm. After the texture surface is completed, a BSG layer is deposited on the front side of the silicon wafer using a tubular device, and the deposition parameters are as follows: at a temperature of 700°C to 800°C, a boron source and an oxygen gas are introduced for deposition for 400 to 600 seconds, and a source-oxygen ratio of 1:3 to 1:5, and a BSG layer with a thickness of 80 to 100 nm is obtained on the texture surface on the front side of the silicon wafer; S2. Inkjet ethyl silicate solution as a barrier layer solution on the surface of the front BSG layer. The ethyl silicate solution includes ethyl silicate and a volatile solvent (such as ethanol, water, or other solvents that can evaporate quickly at the subsequent temperature). Dry at 100-200°C to constant weight (according to the properties of the solvent, the relevant drying time to constant weight is obtained through optimization experiments. In this case, ethanol and water are used with a volume ratio of 9:1 and the drying time is about 30-80s) to form a barrier layer. After drying, the weight increases by 2.0-3.0mg. S3, performing laser film opening treatment on the barrier layer, wherein the laser film opening parameters are: using 532nm pulse laser for film opening, film opening power of 17-30W, and spot size of 110-150μm; S4. Place the opened sample in a low-pressure boron expansion tube for boron expansion treatment. The boron expansion treatment parameters are as follows: temperature set at 950~990℃, pressure set at 150~200mbar, boron source (such as BCl3, BBr3, etc.) and oxygen, source-oxygen ratio 1:3~1:5, deposition time 400~600s, advancement time 3000~5000s. After the boron expansion treatment, a lightly doped area and a heavily doped area are formed. The square resistance of the lightly doped area is 300~400Ω / sq, and the square resistance of the heavily doped area is 70~160Ω / sq, and a silicon wafer containing a selective emitter is obtained. Example 4
[0022] A method for preparing a crystalline silicon cell comprises the following steps: (1) A silicon wafer including a selective emitter prepared in Example 1; (2) using HF solution to remove the BSG layer on the back side of the silicon wafer (deposition will also occur on the back side during the S1 deposition in Example 1), and then performing alkaline polishing (using a sodium hydroxide aqueous solution with a volume fraction of 2-4%, a temperature of 70°C, and alkaline polishing for 480 seconds) until the back side reflectivity is greater than 40%; In LPCVD, a gas phase oxidation method is used to deposit a 1-2 nm tunnel oxide layer on the back of the silicon wafer at a temperature of 500-600°C, and the layer thickness is controlled by controlling the gas flow rate and deposition time; subsequently, silane is deposited at a deposition temperature of 500-600°C to form a 100-120 nm intrinsic amorphous silicon layer, and the layer thickness is controlled by controlling the silane flow rate and deposition time; (3) introducing POCl3 and O2 gases, and completing high-temperature crystallization and phosphorus diffusion at 700-900°C simultaneously, with a diffusion time of 800-1500s, and obtaining a PSG layer on the back; (4) removing the front side coating and surface oxide layer by chain HF on the front side, and then performing surface passivation treatment, wherein the surface passivation treatment is: first using ALD to deposit a 5-8 nm thick aluminum oxide layer on both sides, and then using PECVD to prepare a passivation anti-reflection film layer on both sides, to obtain a 75-80 nm thick front side passivation anti-reflection film layer (silicon nitride film), and a 80-90 nm thick back side passivation anti-reflection film layer (silicon nitride film); (5) Double-sided metallization process to make electrodes: Use screen printing to print silver paste electrodes on the back of the silicon wafer and silver aluminum paste electrodes on the front. After sintering, a back silver electrode and a front aluminum electrode are obtained, thus obtaining an N-type TOPCon crystalline silicon cell. Example 5
[0023] The method for preparing the crystalline silicon cell in this case is the same as that in Example 4, except that step (1) uses the silicon wafer containing the selective emitter of Example 2. Example 6
[0024] The method for preparing the crystalline silicon cell in this case is the same as that in Example 4, except that step (1) uses the silicon wafer containing the selective emitter of Example 3.
[0025] Comparative Example 1 The preparation of the battery in this case is the same as that in Example 4, except that the method of Example 1 is not used to prepare the silicon wafer containing the selective emitter, but the conventional laser direct doping method is used. The specific preparation process is as follows: S1, select N-type single crystal silicon wafer with resistivity of 0.6~2.0Ω·cm, minority carrier lifetime>2.5 ms, thickness of 130±8µm, and size of 182mm×182mm; The damaged layer on the surface of the silicon wafer is removed in a mixed solution of KOH and H2O2, and then double-sided texturing is performed in the KOH solution to form a pyramid velvet surface with a height of 1~3µm. S2. After the velvet surface is completed, the pre-oxidation (780~800℃) + deposition (800~900℃, BCl3 and O2 flow ratio is 1:2~1:5, pressure 100~300mbar) + propulsion (850~950℃) process is carried out in a tubular high-temperature equipment to complete the single-sided low-pressure boron diffusion. After the boron diffusion treatment, the square resistance is 100~250Ω / sq; S3, performing laser local doping treatment on the diffused sample to achieve local heavy doping, and the local square resistance after laser treatment is 30~80Ω / sq; S4. Place the sample after laser treatment in a low-pressure furnace tube for oxidation treatment. The oxidation treatment parameters are as follows: temperature is set at 950°C~1050°C, pressure is set at 400~800mbar, oxygen flow rate is 20000~40000sccm, oxidation time is 3000~4500s. After oxidation treatment, the square resistance of the lightly doped area is 200~400Ω / sq, and the square resistance of the heavily doped area is 100~200Ω / sq, and a silicon wafer containing a selective emitter is obtained.
[0026] Comparative Example 2 The preparation of the battery in this case is the same as that in Example 4, except that: when preparing the silicon wafer containing the selective emitter in Example 1, no barrier layer is prepared.
[0027] The electrical performance of the batteries prepared in the above Examples 4 to 6 and Comparative Examples 1 to 2 was tested. Ten batteries were prepared in each case and the average value was taken. The results are shown in Table 1.
[0028] Table 1 Battery performance of each case Open circuit voltage Uoc (mV) <![CDATA[Short - circuit current density Jsc (mA / m 2 )]]> Fill Factor FF Photoelectric conversion efficiency Eta (%) Example 4 738.5 40.18 85.27 25.32 Comparative Example 1 738.2 40.07 85.21 25.21 Comparative Example 2 736.9 40.10 85.19 25.18 Example 5 739.0 40.14 85.16 25.24 Example 6 736.5 40.16 85.30 25.21 As shown in Table 1, compared with the battery of Example 4, the open circuit voltage and photoelectric conversion efficiency of the battery prepared in Comparative Example 2 without a barrier layer are lower. The battery prepared by the method of Example 4 of the present invention has slightly better electrical performance than the conventional technical solution (Comparative Example 1).
[0029] The barrier layer in the present invention can completely block the subsequent boron diffusion to the lightly doped area, and can avoid the adverse effect on the uniformity of the square resistance of the lightly doped area; the present invention does not need to adopt the reverse etching process, and the method of adopting the barrier layer can better maintain the morphology and light trapping effect of the lightly doped area, while ensuring that the stability of the square resistance of the lightly doped area can be controlled in a more industrialized manner; this patent adopts inkjet of the barrier layer solution to realize the preparation of the barrier layer, which can more flexibly control the thickness of the barrier layer, without considering how to achieve a balance between the thickness of the oxide layer and the laser damage problem by laser oxidation in the prior art.
[0030] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. Method for preparing selective emitter based on low temperature boron diffusion method, It is characterized in that The steps include: S1, taking a double-sided textured silicon wafer, and depositing a BSG layer on the textured surface on the front side of the silicon wafer; S2, inkjet a barrier layer solution on the surface of the BSG layer, and form a barrier layer after drying; S3, performing laser film opening treatment on the barrier layer; S4. The sample after film opening is subjected to boron diffusion treatment. The unopened area is lightly doped to form a lightly doped area due to the presence of the barrier layer, while the opened area is heavily doped to form a heavily doped area due to the absence of the barrier layer, thereby obtaining a silicon wafer containing a selective emitter.
2. The method for preparing a selective emitter based on low temperature boron diffusion method according to claim 1, It is characterized in that The barrier layer solution includes one or more substances selected from the group consisting of silicate, silanol, silicon nitride sol, sodium aluminate, and ammonium sulfate; The barrier layer solution is inkjetted and then dried at 80-200° C. to a constant weight. The barrier layer solution increases in weight by 1-10 mg after being dried.
3. The method for preparing a selective emitter based on low temperature boron diffusion method according to claim 1, It is characterized in that A BSG layer is deposited on the front side of the silicon wafer using a tubular device, and the deposition parameters are as follows: at a temperature of 600-900° C., a mixed gas of a boron source and oxygen is introduced for deposition for 200-600 seconds, and the volume ratio of the boron source to oxygen is 1:2-1:
5.
4. The method for preparing a selective emitter based on low temperature boron diffusion method according to claim 1, It is characterized in that The laser film opening process is to the BSG layer; the laser film opening process uses a pulsed laser to open the film, the film opening power is 10-30W, the spot size is 70-150μm, and the distance between two adjacent film opening areas is determined according to the graphic design requirements.
5. The method for preparing a selective emitter based on low temperature boron diffusion method according to claim 1, It is characterized in that The boron expansion treatment is carried out in a low-pressure boron expansion tube, the temperature is set to 900-1000°C, the pressure is set to 100-300mbar, a mixed gas of a boron source and oxygen is introduced, the volume ratio of the boron source to oxygen is 1:2-1:5, the deposition time is 200-600s, and the advancement time is 1000-5000s.
6. The method for preparing a selective emitter based on low temperature boron diffusion method according to any one of claims 1 to 5, It is characterized in that The silicon wafer is an N-type single crystal silicon wafer; The suede surface is a pyramid structure suede surface; The thickness of the BSG layer is 60-100 nm; The thickness of the barrier layer retained in the lightly doped region is 20-70 nm; The square resistance of the lightly doped region is 200-800Ω / sq, and the square resistance of the heavily doped region is 50-200Ω / sq.
7. Method for preparing crystalline silicon battery, It is characterized in that The steps include: (1) Providing a silicon wafer comprising a selective emitter produced by the production method according to any one of claims 1 to 6; (2) After removing the BSG layer on the back of the silicon wafer and performing alkali polishing, a tunnel oxide layer and an intrinsic amorphous silicon layer are formed on the back in sequence; (3) Then, phosphorus diffusion treatment is performed and crystallization treatment is completed at the same time, and a PSG layer is obtained on the surface; (4) After removing the front and edge plating and surface oxide layer, perform surface passivation treatment; (5) The electrodes are made by double-sided metallization process and then sintered to form crystalline silicon cells.
8. The method for preparing a crystalline silicon cell according to claim 7, It is characterized in that The process conditions for performing phosphorus diffusion treatment and completing crystallization treatment at the same time are: in a mixed gas of phosphorus source gas and oxygen, diffusion is performed at 700-900°C for 800-4000s, so that high-temperature crystallization and phosphorus diffusion can be completed simultaneously; The surface passivation treatment is: firstly, aluminum oxide layers are deposited on both sides by ALD, and then a passivation anti-reflection film layer is prepared on both sides by PECVD.
9. The method for preparing a crystalline silicon cell according to claim 8, It is characterized in that The alkali polishing makes the back reflectivity greater than 40%; the thickness of the tunneling oxide layer is 1~2nm, the thickness of the intrinsic amorphous silicon deposition layer is 50~150nm; the thickness of the aluminum oxide layer is 3~10nm, the thickness of the front passivation anti-reflection film layer is 75~80nm, and the thickness of the back passivation anti-reflection film layer is 70~100nm; the back silver electrode is manufactured by the back metallization process, and the front aluminum electrode is manufactured by the front metallization process.