Novel copper and selenium doping method for CdTe solar cell
By using CuSeCN material to dopate copper and selenium on the back contact surface of CdTe solar cells, the CdSexTe1-x alloy layer is solved, and the problem of difficult to detect and construct alloy layers in the prior art is improved, and the device performance is reduced. The basis barrier achieves more efficient carrier extraction.
Patent Information
- Application Number
- CN202410963698.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to deeply detect and construct the CdSexTe1-x alloy layer in CdTe solar cells, and the high-cost precious metal Au as the back electrode limits the device performance, and the Schottky barrier problem is difficult to completely solve.
CuSeCN material is used to dopant copper and selenium on the back contact surface of CdTe solar cells. Through the preparation of CuSeCN ammonia spin coating solution and thermal activation treatment, a high-performance CdSexTe1-x alloy layer is formed, reducing the Schottky barrier of the device and Improve carrier extraction rate.
The carrier extraction rate is improved, the Schottky barrier is reduced, and the measurable p-type CdSexTe1-x alloy layer is formed, which improves the overall performance of CdTe solar cells and shows that it is more than CuSCN/CdSe double-layer treatment. High efficiency.
Smart Images

Figure CN118969896A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper and selenium doping, in particular to a novel copper and selenium doping method for CdTe solar cells. Background Art
[0002] With the development and large-scale application of the photovoltaic industry, CdTe solar cells are widely used in large-scale industrial production due to their good stability and suitable band gap (1.48eV). The manufacture of high-quality CdTe benefits from the composition / band gap optimization of the absorber layer, for example, by inserting selenium into the front junction position of the absorber layer to form CdSe x Te 1-x Alloy layer. Due to the band bending effect in the CdSe-CdTe system, the intrinsic band gap of CdTe can be reduced from 1.48eV to 1.4eV, which is feasible for broadening the spectral range (300-900nm) and achieving better band alignment of CdSe-CdTe heterostructures. The additional Se atoms show higher solubility in the CdTe absorber relative to S atoms. This is due to the interaction with CdS Compared to the lattice constant of the formed CdSe Closer to the lattice constant of CdTe Therefore, the lattice mismatch at the CdSe / CdTe interface is smaller than that at CdS / CdTe. A great deal of research effort has focused on engineering process parameters to minimize the CdSe x Te 1-x The band gap of CdSe satisfies the optimal band gap in the Shockley-Queisser thermodynamic limit of solar cell efficiency. Theoretical calculations confirm that x Te 1-x The optical band gap of CdSe is less than 1.4 eV, which provides more opportunities for the preparation of absorbers in the future. However, since the current industry is mainly committed to Se doping at the front junction position, it is difficult to deeply detect CdSe under current technical conditions. x Te 1-x The specific optical band gap of the alloy layer. Obviously, the gradient CdTe is constructed over the entire absorber using ex situ doping only at the front junction position. x Se 1-x Very difficult.
[0003] Considering the back structure of the battery, the back contact material is usually based on copper-based materials, such as metallic copper and oxides, halides containing copper ions, etc. This is due to the lack of hole density in CdTe, which usually requires additional hole injection. Cu diffusion has become an important method for preparing high-performance CdTe solar cells and has been widely explored. Therefore, copper-based materials are still the mainstream hole activation engineering. In this regard, in addition to further optimizing the copper doping method, the development of new back contact materials will help to achieve more efficient element doping methods and hole carrier density in the absorber. In addition, the high work function of CdTe itself (~5.3eV) makes it difficult to match a suitable metal electrode, which will greatly limit the carrier transport between the absorption layer and the metal electrode interface. Although all thin-film solar cells usually use various metal films as back electrodes, such as Mo, Au, Ni, Ag, Al and Cu, it is undeniable that many high-efficiency solar cells still cannot do without Au as the back electrode. But as a precious metal, Au has a high industrial cost, which is not conducive to the future competition of the CdTe photovoltaic industry. It is basically impossible to completely solve the Schottky barrier problem by simply replacing the metal electrode. Using semiconductors with lower work functions to replace metal back electrodes can effectively eliminate the Schottky barrier. However, p-type semiconductors with higher work functions are extremely scarce and need further research and development. Therefore, the present invention proposes a novel copper and selenium doping method for CdTe solar cells to solve the problems existing in the prior art. Summary of the invention
[0004] In view of the above problems, the present invention aims to propose a novel copper and selenium doping method for CdTe solar cells, which can realize the Cu activation process on the back contact surface and construct CdSe x Te 1-x The alloy layer was formed and the work function was further reduced. Finally, a measurable p-type CdSe was successfully formed on the back side. x Te 1-x , which greatly improves the overall performance of CdTe batteries and can solve the problems existing in the existing technology.
[0005] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: a novel copper and selenium doping method for CdTe solar cells, comprising the following steps:
[0006] Step 1: Preparation of solar cell back contact layer materials
[0007] Under air conditions, CuSO4·5H2O and Na2S2O3·5H2O are dissolved in DI water and stirred until completely dissolved to obtain a precursor solution. Then, under ice bath conditions, KSeCN is dissolved in DI water and quickly added to the precursor solution, and stirred again for reaction. After the reaction is completed, the off-white precipitate of CuSeCN is collected and purified to obtain CuSeCN powder.
[0008] Step 2: Preparation of CuSeCN ammonia spin coating solution
[0009] Dissolving the CuSeCN powder obtained in step 1 in an ammonia solution to obtain a CuSeCN ammonia spin-coating solution, and then filtering to obtain a clarified CuSeCN ammonia spin-coating solution;
[0010] Step 3: Preparation of thin film on the back surface of solar cells
[0011] Under air conditions, the clarified CuSeCN ammonia solution obtained in step 2 is spin-coated to deposit a p-type CuSeCN film on the back contact surface of the CdTe solar cell. After the deposition of the CdTe solar cell film is completed, a thermal activation treatment is performed to complete the copper activation and obtain high-performance CdSe x Te 1-x Alloy layer.
[0012] A further improvement is that in step 1, the purification treatment method is: the gray-white precipitate is washed with deionized water, ether and ethanol for 1 to 3 times respectively, and then placed in a vacuum oven for drying, wherein the drying temperature is 70 to 80°C and the time is 12 to 16 hours.
[0013] A further improvement is that in step 2, the filtering treatment is carried out by placing the CuSeCN ammonia spin-coating liquid at 50-70° C., stirring for 2-3 hours, and then cooling it. After cooling, filtering is performed using a 0.22 μm filter head.
[0014] A further improvement is that in step 2, the concentration of the CuSeCN ammonia spin coating solution is controlled to be 1-20 mg / mL.
[0015] A further improvement is that in step three, the thermal activation treatment is performed by rapidly heating the deposited thin film.
[0016] A further improvement is that in step 3, the CdSe x Te 1-x The Se doping amount is adjusted to: temperature of 100-300° C., and time of 10-180 min.
[0017] A further improvement is that in step 3, the specific steps of depositing the thin film are:
[0018] A1: Soak the solar cell in diluted hydrochloric acid, rinse the surface with deionized water, and purge the surface with nitrogen;
[0019] A2: Spin coating method was used to cast CuSeCN spin coating solution to prepare the film;
[0020] A3: Annealing process is used to complete the diffusion of Cu and Se and CdSe x Te 1-x Preparation of alloy layer.
[0021] A further improvement is that the film thickness is 100 to 3000 nm.
[0022] A further improvement is that the CdSe x Te 1-x The alloy layer is located on the back contact surface of CdTe and has a band gap smaller than the intrinsic band gap of CdTe.
[0023] The beneficial effects of the present invention are as follows: the novel copper and selenium doping method for CdTe solar cells provided by the present invention develops a new material with dual activation of Cu and Se, improves the carrier extraction rate, reduces the Schottky barrier of the device, and prepares CdSe with a measurable band gap. x Te 1-x The alloy layer exhibited similar hole activation performance as CuSCN. In addition, the CdTe film treated with CuSeCN showed higher efficiency than the device treated with CuSCN / CdSe bilayer. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the material synthesis route of Example 1 of the present invention.
[0025] Figure 2 This is the XRD spectrum of the CuSeCN powder prepared in Example 1 of the present invention.
[0026] Figure 3 This is the XRD spectrum of the CuSeCN film prepared in Example 1 of the present invention.
[0027] Figure 4 This is the device preparation route map of Example 2 of the present invention
[0028] Figure 5 It is the XPS energy spectrum diagram of the CdTe / CuSeCN device and the pure CdTe device prepared in Example 2 of the present invention.
[0029] Figure 6 It is a Tauc plots curve diagram of the films prepared in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention.
[0030] Figure 7 It is the UPS energy spectrum of pure CdTe, the material synthesized in Example 1 of the present invention, and the thin film prepared in Example 2.
[0031] Figure 8 It is the Tauc plots of CuSCN and the material synthesized in Example 1 of the present invention.
[0032] Fig. 9 3 is an energy band structure diagram of the device prepared in Example 2 of the present invention.
[0033] Fig.10 3 is a device structure diagram of the device prepared in Example 2 of the present invention.
[0034] Fig.11 It is a JV curve diagram of the CdTe solar cell of the present invention after copper treatment of different materials.
[0035] Fig.12 It is a schematic diagram of the external quantum efficiency of the devices prepared in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0036] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0037] In the following examples, the materials are purchased from the market. The present invention is based on the basic structure of CdTe solar cells, uses CuSeCN as the back contact layer material, adds it between cadmium telluride and the metal back electrode, and prepares a new device structure. The method involves the synthesis of CuSeCN and the preparation of the back surface film of the CdTe solar cell.
[0038] Embodiment 1
[0039] according to Figure 1-Figure 3 As shown, this embodiment relates to a synthesis method of CuSeCN, such as Figure 1 As shown in the figure, this figure shows the chemical synthesis route of CuSeCN, including the synthesis of powder materials and the preparation of spin coating liquid. All reactions are carried out in an air environment:
[0040] S1: Dissolve 5 g CuSO4·5H2O in a 250 mL conical flask containing 100 mL DI water to form a dark blue solution;
[0041] S2: After the solid is completely dissolved, add 5g of white Na2S2O3·5H2O powder, and the solution turns dark green;
[0042] S3: After the white powder is completely dissolved, transfer the solution to an ice bath and stir while keeping the reaction temperature below 0°C. Then dissolve 1.94 g KSeCN in 10 mL DI water and quickly add it to the above solution. A light red precipitate quickly precipitates from the solution;
[0043] S4: After continuous stirring in an ice bath for 1 h, the final solution turned into a uniform grayish-white turbid liquid;
[0044] S5: After the reaction is completed, the off-white precipitate of CuSeCN is collected and then washed twice with deionized water, ether and ethanol to remove unreacted sulfide;
[0045] S6: After washing, drying in a vacuum oven at 80 °C for 14 h to obtain a gray CuSeCN powder (yield exceeding 80%);
[0046] S7: CuSeCN spin coating solutions are finally obtained by dissolving CuSeCN powders of different masses in 1 mL of ammonia solutions of different concentrations;
[0047] S8: placing the prepared copper cyanate spin coating solution at 60° C. and stirring for 2 h;
[0048] S9: After cooling, filter using a 0.22 μm filter head to obtain a clear spin coating solution.
[0049] Further, such as Figure 2 and Figure 3 As shown in FIG. 1 , the XRD pattern of the CuSeCN material prepared in Example 1 of the present invention. Figure 2 It can be clearly observed that the synthesized powdered CuSeCN was identified as an orthorhombic α-CuSeCN phase. In order to capture its peak signal more clearly, we used spin-coated CuSeCN on a Si substrate for testing, and observed three strong diffraction peaks at 26.0°, 44.8°, and 45.9° at 2θ, marked as I, II, and III, respectively. Figure 3 The final result confirmed that the CuSeCN film was hexagonal wurtzite phase (β-CuSeCN).
[0050] Embodiment 2
[0051] according to Figure 4-Figure 12 As shown, this embodiment relates to a method for preparing CuSeCN related devices, such as Figure 4 As shown in the figure, the detailed preparation process and application of CuSeCN on CdTe devices:
[0052] AA1: The FTO conductive glass was cleaned several times with detergent, DI H2O, acetone, and ethanol and dried with nitrogen;
[0053] AA2: CdSe and CdTe thin films deposited on glass substrates using CSS method;
[0054] AA3: Activation of CdTe devices using CdCl2;
[0055] AA4: Soak the battery in diluted hydrochloric acid (HCl:DI H2O=1:10, V / V) for 1 minute to remove surface oxides;
[0056] AA5: After immersion, rinse the surface with deionized water and purge the surface with nitrogen to remove excess CdCl2 and hydrochloric acid;
[0057] AA6: Casting the film by spin coating, the film was prepared by casting the above CuSeCN spin coating solution, and the film thickness was controlled by using different rotation speeds to obtain the optimal film thickness;
[0058] AA7: Annealing treatment is performed to control the Se and Cu doping amounts in the material by controlling the annealing time and annealing stability;
[0059] AA8: Finally, magnetron sputtering was used to deposit Mo / Al / Cr as the back electrode on the battery, and the active area of the battery was 1cm 3 .
[0060] Embodiment 3
[0061] This embodiment proposes a novel copper and selenium doping method for CdTe solar cells, comprising the following steps:
[0062] Step 1: Preparation of solar cell back contact layer materials
[0063] Under air conditions, CuSO4·5H2O and Na2S2O3·5H2O are dissolved in DI water and stirred until completely dissolved to obtain a precursor solution. Then, under ice bath conditions, KSeCN is dissolved in DI water and quickly added to the precursor solution, and stirred again for reaction. After the reaction is completed, the off-white precipitate of CuSeCN is collected and purified to obtain CuSeCN powder, wherein the purification method is: the off-white precipitate is washed with deionized water, ether and ethanol for 3 times respectively, and then placed in a vacuum oven for drying, wherein the drying temperature is 80°C and the time is 12 hours;
[0064] Step 2: Preparation of CuSeCN ammonia spin coating solution
[0065] The CuSeCN powder obtained in step 1 is dissolved in an ammonia solution to obtain a CuSeCN ammonia spin-coating solution, which is then filtered to obtain a clarified CuSeCN ammonia spin-coating solution. The filtering method is as follows: the CuSeCN ammonia spin-coating solution is placed at 70° C., stirred for 2 hours, and then cooled. After cooling, the solution is filtered using a 0.22 μm filter head to control the concentration of the CuSeCN ammonia spin-coating solution to be 20 mg / mL.
[0066] Step 3: Preparation of thin film on the back surface of solar cells
[0067] Under air conditions, the clarified CuSeCN ammonia solution obtained in step 2 is spin-coated to deposit a p-type CuSeCN film on the back contact surface of the CdTe solar cell. After the deposition of the CdTe solar cell film is completed, a thermal activation treatment is performed to complete the copper activation and obtain high-performance CdSe x Te 1-x The alloy layer, wherein the thermal activation treatment method is: the deposited film is rapidly heated, and the CdSe x Te 1-x The Se doping amount is 100%, wherein the heat treatment is adjusted to: temperature of 300°C, time of 10min, and the specific steps of depositing the film are:
[0068] A1: Soak the solar cell in diluted hydrochloric acid, rinse the surface with deionized water, and purge the surface with nitrogen;
[0069] A2: The CuSeCN spin coating solution was cast by spin coating to prepare the film, and the film thickness was 3000nm.
[0070] A3: Annealing process is used to complete the diffusion of Cu and Se and CdSe x Te 1-x Preparation of alloy layer.
[0071] CdSe x Te 1-x The alloy layer is located on the back contact surface of CdTe and has a band gap smaller than the intrinsic band gap of CdTe.
[0072] Embodiment 4
[0073] This embodiment proposes a novel copper and selenium doping method for CdTe solar cells, comprising the following steps:
[0074] Step 1: Preparation of solar cell back contact layer materials
[0075] Under air conditions, CuSO4·5H2O and Na2S2O3·5H2O were dissolved in DI water and stirred until completely dissolved to obtain a precursor solution. Then, KSeCN was dissolved in DI water under ice bath conditions and quickly added to the precursor solution, and stirred again for reaction. After the reaction was completed, the off-white precipitate of CuSeCN was collected and purified to obtain CuSeCN powder. The purification method was as follows: the off-white precipitate was washed once with deionized water, ether and ethanol respectively, and then placed in a vacuum oven for drying, wherein the drying temperature was 70°C and the time was 16 hours;
[0076] Step 2: Preparation of CuSeCN ammonia spin coating solution
[0077] The CuSeCN powder obtained in step 1 is dissolved in an ammonia solution to obtain a CuSeCN ammonia spin-coating liquid, which is then filtered to obtain a clarified CuSeCN ammonia spin-coating liquid, wherein the filtering method is as follows: the CuSeCN ammonia spin-coating liquid is placed at 50° C., stirred for 3 hours, and then cooled, and after cooling, filtered using a 0.22 μm filter head to control the concentration of the CuSeCN ammonia spin-coating liquid to be 1 mg / mL;
[0078] Step 3: Preparation of thin film on the back surface of solar cells
[0079] Under air conditions, the clarified CuSeCN ammonia solution obtained in step 2 is spin-coated to deposit a p-type CuSeCN film on the back contact surface of the CdTe solar cell. After the deposition of the CdTe solar cell film is completed, a thermal activation treatment is performed to complete the copper activation and obtain high-performance CdSe x Te 1-x The alloy layer, wherein the thermal activation treatment method is: the deposited film is rapidly heated, and the CdSe x Te 1-x The Se doping amount is , wherein the heat treatment is adjusted as follows: temperature is 100°C and time is 180min.
[0080] In step 3, the specific steps of depositing the thin film are:
[0081] A1: Soak the solar cell in diluted hydrochloric acid, rinse the surface with deionized water, and purge the surface with nitrogen;
[0082] A2: Spin coating was used to cast CuSeCN spin coating solution to prepare the film, and the film thickness was 100nm;
[0083] A3: Annealing process is used to complete the diffusion of Cu and Se and CdSe x Te 1-x Preparation of alloy layer.
[0084] CdSe x Te 1-x The alloy layer is located on the back contact surface of CdTe and has a band gap smaller than the intrinsic band gap of CdTe.
[0085] Embodiment 5
[0086] This embodiment proposes a novel copper and selenium doping method for CdTe solar cells, comprising the following steps:
[0087] Step 1: Preparation of solar cell back contact layer materials
[0088] Under air conditions, CuSO4·5H2O and Na2S2O3·5H2O were dissolved in DI water and stirred until completely dissolved to obtain a precursor solution. Then, KSeCN was dissolved in DI water under ice bath conditions and quickly added to the precursor solution, and stirred again for reaction. After the reaction was completed, the off-white precipitate of CuSeCN was collected and purified to obtain CuSeCN powder. The purification method was as follows: the off-white precipitate was washed twice with deionized water, ether and ethanol respectively, and then placed in a vacuum oven for drying, wherein the drying temperature was 80°C and the time was 14 hours;
[0089] Step 2: Preparation of CuSeCN ammonia spin coating solution
[0090] The CuSeCN powder obtained in step 1 is dissolved in an ammonia solution to obtain a CuSeCN ammonia spin-coating solution, which is then filtered to obtain a clarified CuSeCN ammonia spin-coating solution. The filtering method is as follows: the CuSeCN ammonia spin-coating solution is placed at 60° C., stirred for 2 hours, and then cooled. After cooling, the solution is filtered using a 0.22 μm filter head, wherein the concentration of the CuSeCN ammonia spin-coating solution is controlled to be 10 mg / mL;
[0091] Step 3: Preparation of thin film on the back surface of solar cells
[0092] Under air conditions, the clarified CuSeCN ammonia solution obtained in step 2 is spin-coated to deposit a p-type CuSeCN film on the back contact surface of the CdTe solar cell. After the deposition of the CdTe solar cell film is completed, a thermal activation treatment is performed to complete the copper activation and obtain high-performance CdSe x Te 1-x The alloy layer, wherein the thermal activation treatment method is: the deposited film is rapidly heated, and the CdSe x Te 1-x The Se doping amount is , wherein the heat treatment is adjusted as follows: temperature is 200°C and time is 110min.
[0093] In step 3, the specific steps of depositing the thin film are:
[0094] A1: Soak the solar cell in diluted hydrochloric acid, rinse the surface with deionized water, and purge the surface with nitrogen;
[0095] A2: Spin coating was used to cast CuSeCN spin coating solution to prepare the film, and the film thickness was 1000nm;
[0096] A3: Annealing process is used to complete the diffusion of Cu and Se and CdSe x Te 1-x Preparation of alloy layer.
[0097] CdSe x Te 1-x The alloy layer is located on the back contact surface of CdTe and has a band gap smaller than the intrinsic band gap of CdTe.
[0098] Comparative Example 1
[0099] This comparative example relates to a method for preparing a CdTe device based on CuCl2 treatment, with detailed preparation process and application:
[0100] SS1: The FTO conductive glass was cleaned several times with detergent, DI H2O, acetone, and ethanol and dried with nitrogen;
[0101] SS2: CdSe and CdTe thin films are deposited on glass substrates using the CSS method;
[0102] SS3: Activation treatment of CdTe devices using CdCl2;
[0103] SS4: Soak the battery in diluted hydrochloric acid (HCl:DI H2O=1:10, V / V) for 1 minute to remove surface oxides;
[0104] SS5: After immersion, rinse the surface with deionized water and purge the surface with nitrogen to remove excess CdCl2 and hydrochloric acid;
[0105] SS6: Prepare CuCl2 solution by dissolving 0.058 mol of CuCl2·2H2O in 1 mL of DI water;
[0106] SS7: Casting the film by spin coating, preparing the film by casting the above CuCl2 spin coating solution, and controlling the film thickness by using different rotation speeds to obtain the optimal film thickness;
[0107] SS8: Annealing treatment is performed to control the Cu doping amount in the material by controlling the annealing time and annealing stability;
[0108] SS9: Finally, magnetron sputtering was used to deposit Mo / Al / Cr as the back electrode on the battery, and the active area of the battery was 1cm 3 .
[0109] Comparative Example 2
[0110] This comparative example relates to a method for preparing a CdTe device based on CuSCN treatment, with detailed preparation process and application:
[0111] B1: Use detergent, DI H2O, acetone, and ethanol to clean the FTO conductive glass several times and blow dry it with nitrogen;
[0112] B2: CdSe and CdTe thin films are deposited on a glass substrate using the CSS method;
[0113] B3: Activate the CdTe device with CdCl2;
[0114] B4: Soak the battery in diluted hydrochloric acid (HCl:DI H2O=1:10, V / V) for 1 minute to remove surface oxides;
[0115] B5: After immersion, rinse the surface with deionized water and purge the surface with nitrogen to remove excess CdCl2 and hydrochloric acid;
[0116] B6: CuSCN spin coating solution was finally obtained by dissolving different masses of CuSCN powder in 1 mL of ammonia solution with different concentrations;
[0117] B7: Casting the film by spin coating, preparing the film by casting the above CuSCN spin coating solution, and controlling the film thickness by using different rotation speeds to obtain the optimal film thickness;
[0118] B8: Perform annealing treatment to control the Cu doping amount in the material by controlling the annealing time and annealing stability;
[0119] B9: Finally, magnetron sputtering was used to deposit Mo / Al / Cr as the back electrode on the battery. The effective area of the battery was 1cm 3 .
[0120] Comparative Example 3
[0121] This comparative example relates to a method for preparing a CdTe device based on CuSCN / CdSe processing, with detailed preparation process and application:
[0122] C1: The FTO conductive glass was cleaned several times with detergent, DI H2O, acetone, and ethanol and dried with nitrogen;
[0123] C2: CdSe and CdTe thin films are deposited on glass substrates using the CSS method;
[0124] C3: Activate the CdTe device with CdCl2;
[0125] C4: Soak the battery in diluted hydrochloric acid (HCl:DI H2O=1:10, V / V) for 1 minute to remove surface oxides;
[0126] C5: After immersion, rinse the surface with deionized water and purge the surface with nitrogen to remove excess CdCl2 and hydrochloric acid;
[0127] C6: CuSCN spin coating solution was finally obtained by dissolving different masses of CuSCN powder in 1 mL of ammonia solution with different concentrations;
[0128] C7: Casting the film by spin coating, preparing the film by casting the above CuSCN spin coating solution, and controlling the film thickness by using different rotation speeds to obtain the optimal film thickness;
[0129] C8: After the spin coating step, it was transferred to an RF magnetron sputtering device and a high-purity CdSe target (99.999%, CNBM Chengdu) was used to deposit a CdSe film with a sputtering pressure of 4 m Torr and a sputtering power of 120 W. The thickness of the CdSe film was controlled by controlling the sputtering deposition time.
[0130] C9: Perform annealing treatment to control the doping amount of Cu and Se in the material by controlling the annealing time and annealing stability;
[0131] C10: Finally, magnetron sputtering was used to deposit Mo / Al / Cr as the back electrode on the battery, and the active area of the battery was 1cm 3 .
[0132] In combination with Embodiments 1 to 5, and Comparative Examples 1 to 3, Figure 5 As shown in the figure, the XPS spectrum of the device prepared in Example 2 of the present invention. A new characteristic peak (binding energy position is 53.7 eV) is also detected in the corresponding battery sample, which is the characteristic peak of Cd-Se. This proves that Se in CuSeCN diffuses in the absorption layer and forms P-type CdSe x Te 1-x It is obvious that the original CdTe film has only noise signals, while the treated sample has obvious characteristic peaks of Se element.
[0133] In order to further illustrate the effect of this selenium doping method on the band gap of the CdTe absorber layer, UV-visible absorption photovoltaic tests and energy band calculations were performed on CdTe devices with different treatments. Figure 6 In ac, the band gaps of untreated and CuSCN-treated CdTe are 1.487 eV and 1.487 eV, respectively. Very different, the band gaps of CdTe / CuSCN / CdSe and CdTe / CuSeCN samples are red-shifted to 1.451 eV and 1.438 eV, which proves the successful preparation of CdSe x Te 1-x But it is clear that CuSeCN can produce a smaller band gap, and the reduction of the CdTe absorber band gap will help broaden the absorption range of the device, thereby greatly improving the current density.
[0134] The energy levels of pure CdTe, CdTe / CuSeCN and CuSeCN were studied by ultraviolet photoelectron spectroscopy (UPS) measurements. Figure 7 ac). The Fermi level positions of CdTe, CdTe / CuSeCN and CuSeCN are -5.22eV, -4.75eV and -4.28eV respectively. The valence band top positions of CdTe, CdTe / CuSeCN and CuSeCN are -5.35eV, -4.86eV and -4.79eV respectively. Combined with the absorption of the sample (as shown in Figure 8 ac), the position of the bottom of the conduction band can be determined, and the energy band structure diagram of the device can be drawn according to the final calculation results (as shown in Fig. 9 As shown). The work function of the original CdTe (5.22eV) is significantly greater than that of the metal electrode Mo (4.6eV), which will produce a Schottky barrier and lead to more charge recombination and energy loss. The work function of the CuSeCN material is (4.28eV), which can prevent direct contact between CdTe and Mo metal electrodes to form an ohmic contact, which means that more carriers will be transferred to the metal electrode and improve the current performance of the solar cell.
[0135] like Fig.10 As shown, the structure of the CuSeCN treated CdTe thin film device is glass / FTO / CdSe /
[0136] CdTe / CuSeCN / Mo / Al / Cr. The preparation of high-quality CdSeTe alloy layers is the key to preparing high-performance CdTe solar cells. After annealing, the Se elements from CuSeCN and CdSe will diffuse into the CdTe absorption layer accordingly, and the final device structure is glass / FTO / CdSe / n-CdSeTe / CdTe / p-CdSeTe(Cu) / CuSeCN / Mo / Al / Cr. CuSeCN can not only adjust the band gap without affecting the overall device performance, but also introduce Se elements well on the back of the absorption layer. Finally, through the bidirectional doping of CdSe and CuSeCN, Se atoms gradually diffuse and distribute on the front and back surfaces of the CdTe layer, which is conducive to capturing more photons. Specifically, due to the influence of CuSeCN, the top CdSeTe is biased toward p-type, while due to the presence of CdSe, the bottom CdSe is biased toward n-type. This quasi-homojunction cell structure can deepen the thickness of the CdSeTe alloy layer in the absorber, which not only broadens the absorption range of the cell but also alleviates the interface lattice strain caused by the lattice matching of CdSe and CdTe.
[0137] Table 1 and Fig.11The photoelectric performance of CdTe solar cells after copper treatment with three different materials: conventional CuCl2, CuSCN and CuSeCN: open circuit voltage (V oc ), short-circuit current density (J sc ), fill factor (FF), conversion efficiency (PCE), series resistance (R s ), parallel resistance (R sh ) and other device parameters. It is obvious that the Jsc and FF of the solar cells treated with CuSeCN increased significantly compared with those of the devices treated with traditional materials such as CuCl2 and CuSCN, resulting in an increase in PCE from 13.40% and 15.15% to 17.48%, respectively. The effective photoelectric conversion efficiency shows that CuSeCN can effectively complete the copper expansion process, V oc The significant enhancement of FF and J indicates that the addition of new carrier transport materials to the original device can effectively passivate defects and enhance carrier extraction. The performance of the CuSeCN treatment results is similar. After CuSCN treatment, the cell is Se-doped with CdSe, and the device's J sc Enhanced to 30.02mA / cm 2 , thanks to CdSe x Te 1-x The formation of the alloy layer leads to the broadening of the spectral absorption. CdSe is used as a Se doping source, and the doping amount of CdSe is extremely limited, reaching only 20nm. This is attributed to CdSe as an n-type material, which seriously affects the transmission of the device and makes it difficult to construct a p-CdSeTe alloy layer by doping a large amount of CdSe on the back of the battery. Therefore, its impact on performance is far less than that of CuSeCN.
[0138] Fig.12 The external quantum efficiency (EQE) of the device is shown. Due to Se doping, for CdTe / CuCl2 and CdTe / CuSCN samples, the EQE curves of CdTe / CuSCN / CdSe and CdTe / CuSeCN are red-shifted as the absorption of the absorption layer broadens. This further proves that CdSe x Te 1-x Spectral absorption broadening caused by the formation of the alloy layer. It is obvious that Se can cause red-shift and broadening of the absorption and spectral transition of CdTe, but CuSeCN is more significant.
[0139] The present invention can realize ohmic contact in CdTe solar cells, broaden the absorption spectrum of solar cells, and reduce interface recombination. The electrical performance test results of CdTe solar cells with CuSeCN are as follows: the current density is significantly increased, the fill factor is improved, and the open circuit voltage is also increased. Since other copper acceptor dopants are not used in the present invention, this method shows efficient copper expansion characteristics and can be used as an effective replacement material for future copper doping processes. Table 1 shows the photoelectric performance of CdTe solar cells after copper treatment with three different materials: conventional CuCl2, CuSCN and CuSeCN: open circuit voltage (V oc ), short-circuit current density (J sc ), fill factor (FF), conversion efficiency (PCE), series resistance (R s ), parallel resistance (R sh ) and other device parameters, among which, Table 1 is as follows:
[0140]
[0141] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the framework and scope of application of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A novel copper and selenium doping method for CdTe solar cells, characterized in that: The following steps are involved: Step 1: Preparation of solar cell back contact layer materials Under air conditions, CuSO4·5H2O and Na2S2O3·5H2O are dissolved in DI water and stirred until completely dissolved to obtain a precursor solution. Then, under ice bath conditions, KSeCN is dissolved in DI water and quickly added to the precursor solution, and stirred again for reaction. After the reaction is completed, the off-white precipitate of CuSeCN is collected and purified to obtain CuSeCN powder. Step 2: Preparation of CuSeCN ammonia spin coating solution Dissolving the CuSeCN powder obtained in step 1 in an ammonia solution to obtain a CuSeCN ammonia spin-coating solution, and then filtering to obtain a clarified CuSeCN ammonia spin-coating solution; Step 3: Preparation of thin film on the back surface of solar cells Under air conditions, the clarified CuSeCN ammonia solution obtained in step 2 is spin-coated to deposit a p-type CuSeCN film on the back contact surface of the CdTe solar cell. After the deposition of the CdTe solar cell film is completed, a thermal activation treatment is performed to complete the copper activation and obtain high-performance CdSe x Te 1-x Alloy layer.
2. A novel copper and selenium doping method for CdTe solar cells according to claim 1, characterized in that: In the step 1, the purification treatment is as follows: the off-white precipitate is washed with deionized water, ether and ethanol for 1 to 3 times respectively, and then placed in a vacuum oven for drying, wherein the drying temperature is 70 to 80° C. and the drying time is 12 to 16 hours.
3. A novel copper and selenium doping method for CdTe solar cells according to claim 1, characterized in that: In the step 2, the filtering treatment is carried out by placing the CuSeCN ammonia spin coating solution at 50-70° C., stirring for 2-3 hours, and then cooling it. After cooling, filtering is performed using a 0.22 μm filter head.
4. A novel copper and selenium doping method for CdTe solar cells according to claim 1, characterized in that: In the step 2, the concentration of the CuSeCN ammonia spin coating solution is controlled to be 1-20 mg / mL.
5. A novel copper and selenium doping method for CdTe solar cells according to claim 1, characterized in that: In the step three, the thermal activation treatment is performed by rapidly heating the deposited thin film.
6. A novel copper and selenium doping method for CdTe solar cells according to claim 1, characterized in that: In step 3, the CdSe x Te 1-x The Se doping amount is adjusted to: temperature of 100-300° C., and time of 10-180 min.
7. A novel copper and selenium doping method for CdTe solar cells according to claim 1, characterized in that: In step 3, the specific steps of depositing the thin film are: A1: Soak the solar cell in diluted hydrochloric acid, rinse the surface with deionized water, and purge the surface with nitrogen; A2: Spin coating method was used to cast CuSeCN spin coating solution to prepare the film; A3: Annealing process is used to complete the diffusion of Cu and Se and CdSe x Te 1-x Preparation of alloy layer.
8. A novel copper and selenium doping method for CdTe solar cells according to claim 7, characterized in that: The film thickness is 100 to 3000 nm.
9. A novel copper and selenium doping method for CdTe solar cells according to claim 7, characterized in that: The CdSe x Te 1-x The alloy layer is located on the back contact surface of CdTe and has a band gap smaller than the intrinsic band gap of CdTe.