Application of HNBR as lithium ion battery positive electrode binder, lithium ion battery positive electrode and lithium ion battery
By using specific HNBR binders, the problem of insufficient stability of the positive electrode of lithium-ion battery under high voltage conditions is solved, and higher battery performance and environmental protection are achieved. It is suitable for a variety of positive electrode materials, improving the overall performance of the battery.
Patent Information
- Application Number
- CN202411443104.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-ion battery positive electrode adhesive is insufficient in high voltage conditions, resulting in poor battery performance. The fluorine pollution problem limits its sustainable development. It is necessary to develop new adhesives that are resistant to high voltage, high performance, fluorine-free and environmentally friendly. Catheter.
Hydrogenated nitrile rubber (HNBR) with hydrogenation saturation of ≥90%, ACN content of 26%-29%, and Mooney's viscosity ML (1+4)@100℃ is 20-45 as the positive electrode binder for lithium-ion batteries. Suitable for a variety of positive electrode materials, and improves the high voltage performance of the battery by optimizing the structural characteristics of HNBR.
The HNBR binder maintains excellent stability and adhesion under high voltage conditions, improves the charging and discharging efficiency and cycle stability of lithium-ion batteries, reduces side reactions, and promotes the upgrading of high-voltage lithium-ion battery technology.
Smart Images

Figure CN118970056A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy battery materials, and specifically relates to application of HNBR as a positive electrode binder for lithium ion batteries, a positive electrode slurry for lithium ion batteries and a lithium ion battery. Background Art
[0002] As lithium-ion batteries continue to strengthen their core position in electric vehicles, portable electronic devices, and large-scale energy storage, the market has put forward higher standards for their comprehensive performance and economic and environmental benefits. The comprehensive performance of the battery depends not only on the electrode active material, but also closely related to other components. As a key component connecting the active material particles and the current collector, the binder largely determines the stability and durability of the electrode microstructure. Polyvinylidene fluoride (PVDF) is currently the main binder for lithium-ion battery positive electrode materials. It has stable performance and is easy to process, but the serious fluorine pollution during production and use and the problems in lithium ion conductivity limit its sustainable development in the battery industry, and gradually become an urgent problem to be solved and optimized. Therefore, the development of new binders that are resistant to high voltage, high performance, fluorine-free and environmentally friendly has become a difficult problem that academia and industry are working hard to overcome.
[0003] New binders used in high-voltage positive electrodes should have excellent stability, wettability and bonding ability in a wide temperature range and high voltage environment. Hydrogenated nitrile rubber (HNBR) has excellent high / low temperature resistance, corrosion resistance, wettability and adhesion, and is fluorine-free, environmentally friendly and relatively stable, with great application potential. The current patented technology of HNBR applied to lithium-ion battery binders mainly includes three aspects: ① By adjusting the hydrogen saturation of HNBR or introducing functional groups such as nitrile (-CN) to enhance heat resistance and oxidation resistance, or improve the interface compatibility and adhesion with active substances; ② By reasonably matching fillers, cross-linking agents, conductive additives, etc. to optimize conductivity, mechanical properties and processing properties; ③ Adaptability optimization for special applications: for example, specific application strategies and technical solutions in fast charging and discharging, wide temperature operating range, and high-safety battery systems.
[0004] The currently published patents mainly focus on the effect of binders on the slurry (such as slurry stability, adhesion, internal resistance) or electrode sheets (such as conductivity, adhesion strength) of lithium-ion batteries. The quality of the slurry and electrode sheet properties is related to the uniformity of the interface contact and the properties of the binder itself (such as molecular structure, molecular weight and distribution, resistance). However, the quality of the slurry and electrode sheet cannot directly determine the performance of lithium-ion batteries, because lithium-ion batteries have additional requirements for the physicochemical properties of the binder (especially chemical stability and wettability with the electrolyte). For example, the positive electrode of a lithium-ion battery requires the binder to have good resistance to electrochemical oxidation. If the binder's antioxidant capacity is insufficient, when charging at a high voltage (>3.8 V), it will be robbed of electrons by the high oxidation state on the surface of the positive electrode, thereby being oxidized, decomposed, and losing its original function. When the positive electrode material contains elements such as Co and Ni, additional electrocatalytic oxidation processes may also be involved, exacerbating the oxidation of the binder, so higher requirements are placed on the antioxidant capacity of the binder.
[0005] In addition, the relevant patents have a very broad scope of protection for HNBR, such as hydrogen saturation of 50%-100%, acrylonitrile (ACN) content of 16%-50%, Mooney viscosity ML (1+4) @ 100 ° C of 50-120, or molecular weight Mw of 250000-700000, and there is a lack of experimental data to support its role in promoting battery performance. Although the relevant patents have proposed rights protection for the characteristics of HNBR suitable for electrode slurry or electrode sheets, the applicant of the present invention has found in the research that HNBR with some or all of the above characteristics is of various types, with very different physical and chemical properties, and presents huge differences in battery performance when matching different positive electrode materials. This also proves that the quality of slurry and electrode sheets cannot directly determine the performance of lithium-ion batteries, and lithium-ion batteries have additional requirements for the physical and chemical properties of binders. This means that different positive electrode materials need to match different types of HNBR, which imposes a great burden on both production processes and preparation costs. Therefore, it is urgent to develop some special HNBR binders suitable for a variety of positive electrode materials and examine the influence of HNBR structure on battery performance, especially on high voltage performance. Summary of the invention
[0006] The purpose of the present invention is to provide an application of HNBR as a positive electrode binder for a lithium ion battery, a positive electrode for a lithium ion battery and a lithium ion battery.
[0007] In a first aspect, the present invention provides an application of HNBR as a positive electrode binder for lithium-ion batteries;
[0008] The HNBR has a hydrogenation saturation of ≥90%, an ACN content of 26%-29%, and a Mooney viscosity ML (1+4) @ 100°C of 20-45.
[0009] This screened and optimized HNBR binder can maintain excellent stability and adhesion under high voltage conditions and is suitable for a variety of positive electrode materials.
[0010] Preferably, in the lithium-ion battery, the HNBR is used alone as a positive electrode binder.
[0011] Preferably, the hydrogenation saturation of the HNBR is ≥95%, and a more preferred hydrogenation saturation is >99%.
[0012] Preferably, the Mooney viscosity ML (1+4) @ 100°C is 40-45.
[0013] As a further preference, the ACN content of the HNBR is 26%-29%, the hydrogen saturation is >99%, and the Mooney viscosity number ML (1+4) @ 100°C is 40-45.
[0014] In a second aspect, the present invention provides a lithium ion battery positive electrode, which is obtained by uniformly coating a lithium ion battery positive electrode slurry on a current collector and then drying it; the lithium ion battery positive electrode slurry comprises a positive electrode active material, a binder, a conductive agent and a solvent, the binder is HNBR, the hydrogenation saturation of the HNBR is ≥90%, the ACN content is 26%-29%, and the Mooney viscosity ML (1+4) @ 100 ° C is 20-45.
[0015] Preferably, the hydrogenation saturation of the HNBR is ≥95%, and a more preferred hydrogenation saturation is >99%.
[0016] Preferably, the Mooney viscosity ML (1+4) @ 100°C is 40-45.
[0017] As a further preference, the ACN content of the HNBR is 26%-29%, the hydrogen saturation is >99%, and the Mooney viscosity number ML (1+4) @ 100°C is 40-45.
[0018] Preferably, the mass ratio of the positive electrode active material, the binder and the conductive agent is (70-92): (4-15): (4-15), and more preferably 8:1:1.
[0019] Preferably, the positive electrode active material is lithium iron phosphate (LFP), lithium manganese phosphate, lithium cobalt phosphate, lithium manganese iron phosphate, lithium nickel iron phosphate, lithium manganese cobalt phosphate, lithium cobalt oxide (LCO), lithium cobalt manganese oxide, lithium nickel cobalt manganese oxide (Li 10 Ni x Co y Mn z O 20, referred to as NCMxyz, x, y, z are one or more of the molar ratios of nickel, cobalt and manganese (x=2-8, y=1-5, z=1-5, satisfying x+y+z=10), preferably LFP, LCO, lithium nickel cobalt manganese oxide (NCM523), or lithium cobalt manganese oxide, more preferably LFP, LCO, or lithium nickel cobalt manganese oxide (NCM523).
[0020] Preferably, the conductive agent is one or more of conductive carbon black, carbon fiber, and carbon nanotubes, preferably conductive carbon black or carbon nanotubes, and more preferably conductive carbon black.
[0021] Preferably, the solvent is one or more of N-methyl-2-pyrrolidone (NMP), acetone, ethylene glycol dimethyl ether, and anisole, preferably NMP, ethylene glycol dimethyl ether, or anisole, and more preferably NMP.
[0022] Preferably, the current collector is a metal foil or a metal mesh porous sheet, preferably an aluminum foil or a copper foil that has been subjected to a carbon coating.
[0023] In a third aspect, the present invention provides a lithium ion battery, wherein the positive electrode of the lithium ion battery is the positive electrode described in the second aspect.
[0024] According to the above solution, the lithium ion battery is a liquid lithium ion battery or a solid lithium ion battery.
[0025] According to the above scheme, the lithium-ion battery can be assembled into a button battery, a soft-pack battery or a cylindrical battery.
[0026] Preferably, the lithium-ion battery is a liquid lithium-ion battery, and the separator used is one of a polyethylene microporous membrane, a glass fiber membrane or a polypropylene microporous membrane, and more preferably is a polypropylene microporous membrane Celgard 2400.
[0027] Preferably, the lithium-ion battery is a liquid lithium-ion battery, and the electrolyte is composed of a lithium salt, a solvent and an additive, wherein the solvent is one or more of propylene carbonate, ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and diethyl carbonate, and more preferably a mixed solution of EC:EMC:DMC (1:1:1, volume ratio); the lithium salt is one or more of LiFP6, LiBF4, LiAsF4, LiClO4, LiFSI, LiTFSI, and LiNO3, and more preferably LiFP6; the additive is one or more of LiTFSI, lithium difluorooxalatoborate (LiDFOB), allyl pentafluorobenzene (APFB), 2,3,4,5,6-pentafluorophenylboric acid (PFPBA), fluoroethylene carbonate (FEC), lithium bis(oxalatoborate), 4-bromoanisole, and trifluoroethylphosphite, and preferably LiTFSI and / or LiDFOB. It is further preferred that in the electrolyte, the concentration of lithium salt is 0.7-1.5 M, and the concentration of additive is 0.5-2.0% of the concentration of lithium salt.
[0028] Preferably, the lithium-ion battery is a solid-state lithium-ion battery, the solid electrolyte is composed of a lithium salt, a polymer and an additive, the polymer is one of polyvinyl ethylene carbonate (PVEC) and polyethylene oxide (PEO); the lithium salt is one or more of LiFP6, LiBF4, LiAsF4, LiClO4, LiFSI, LiTFSI, LiNO3, more preferably LiTFSI; the additive is one or more of lithium difluorooxalatoborate (LiDFOB), allyl pentafluorobenzene (APFB), 2,3,4,5,6-pentafluorophenylboric acid (PFPBA), fluoroethylene carbonate (FEC), succinonitrile (SN), lithium bisoxalatoborate, 4-bromoanisole, trifluoroethylphosphite, preferably LiDFOB, APFB, PFPBA and SN. It is further preferred that the lithium salt concentration in the electrolyte is 0.7-1.5 M, and the additive concentration is 0.5-2.0%.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] ① A specific HNBR binder is proposed, which is suitable for a variety of lithium-ion battery positive electrode materials;
[0031] ② When this type of binder is used in lithium-ion batteries, it exhibits more environmentally friendly safety and better overall performance than the current fluorine-containing PVDF positive electrode materials. It not only effectively enhances the binding force between the active material and the current collector, improves the battery's charge and discharge efficiency, cycle stability and service life, but also reduces the side reactions of the battery under high-voltage operating conditions, which is of great value in promoting the technological upgrading of high-voltage lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is the molecular structure diagram of HNBR material;
[0033] Figure 2 Characterization / testing procedures and key technical points of the samples described in Comparative Examples 1-3 and Examples 1-9;
[0034] Figure 3 The effect of different ACN contents on the performance of the HNBR-LFP electrode described in Example 1;
[0035] Figure 4 The effect of different hydrogen saturations on the performance of the HNBR-LFP electrode described in Example 2;
[0036] Figure 5 The effect of different Mooney numbers on the performance of the HNBR-LFP electrode described in Example 3;
[0037] Figure 6 The effect of different ACN contents on the performance of the HNBR-LCO electrode described in Example 4;
[0038] Figure 7 The effect of different hydrogen saturations on the performance of the HNBR-LCO electrode described in Example 5;
[0039] Figure 8 The effect of different Mooney numbers on the performance of the HNBR-LCO electrode described in Example 6;
[0040] Fig. 9 The effect of different ACN contents on the performance of the HNBR-NCM523 electrode described in Example 7;
[0041] Fig.10 The effect of different hydrogen saturations on the performance of the HNBR-NCM523 electrode described in Example 8;
[0042] Fig.11 The effect of different Mooney numbers on the performance of the HNBR-NCM523 electrode described in Example 9. DETAILED DESCRIPTION
[0043] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings, but the implementation manner of the present invention is not limited thereto.
[0044] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained by conventional technical means or purchased commercially.
[0045] Figure 1The molecular structure diagram of HNBR is shown. It is obtained by a copolymer of acrylonitrile (ACN) and butadiene through a specific hydrogenation treatment, and the number of carbon-carbon double bonds in the molecular chain is relatively small. The HNBR material involved in the present invention is customized, processed or provided by Zansheng Technology Co., Ltd.
[0046] The preparation process of HNBR is as follows: under nitrogen replacement conditions, add some nitrile rubber and 500mL of anhydrous chlorobenzene to a 1L stainless steel reactor to make the mass concentration of the resulting solution 9%-13%. After complete dissolution under nitrogen sealing conditions, add "Jan's catalyst" (dosage is 0.08~0.13wt% of nitrile rubber), and heat to 60-100℃ (temperature 1) under nitrogen protection for degradation reaction for 0.5-2.0 hours (time 1), and the pressure is 1.0MPa. After adding hydrogen until the pressure reaches 8.0-8.5MPa (pressure 2), heat to 140~150℃ (temperature 2), react for 3-6 hours (time 2), and obtain a liquid HNBR solution. It is precipitated with methanol and vacuum dried at 110℃ to obtain HNBR. The ACN content in the obtained HNBR is consistent with the ACN content in the raw nitrile rubber, so different HNBR samples need to use nitrile rubber raw materials with corresponding ACN content. The specific preparation conditions of the HNBR sample used in the present invention are shown in Table 1.
[0047] Table 1 details the three key indicators of ACN content, hydrogen saturation and Mooney viscosity of samples 1-10 described in Examples 1-9. Among them, the ACN content is between 18% and 45%, the hydrogen saturation is 90%-99.9%, and the Mooney viscosity is between 20 and 85, covering the most representative HNBR types.
[0048] Table 1 Product parameters and preparation conditions of samples 1-10 described in Examples 1-9
[0049]
[0050] Figure 2 The characterization / battery performance test process and key technical points of the samples described in Comparative Examples 1-3 and Examples 1-9 are shown, including four parts: HNBR characterization, pole piece preparation, battery assembly, and performance test. In order to ensure the rigor of the comparative analysis, in addition to the factors to be compared, strict consistency is adopted in the three links of pole piece preparation, battery assembly, and performance test of Comparative Examples 1-3 and Examples 1-9. The specific operation is as follows.
[0051] ① Preparation of pole pieces: Take the positive electrode active material (LFP, LCO or NCM523), binder (PVDF or HNBR) and conductive carbon black in a mass ratio of 8:1:1 and mix and grind in an appropriate amount of NMP solvent to obtain a uniform slurry. The slurry is evenly coated on the carbon-coated aluminum foil with a coating thickness of 50 μm. After vacuum drying at 120°C for 12 h, it is cut into positive pole pieces with a diameter of 12 mm and placed in a glove box for use.
[0052] ②Battery assembly: The prepared positive electrode sheet was assembled into a liquid button cell in an argon-filled glove box (O2 and H2O contents were both <0.1ppm) in the order of negative electrode shell, spring gasket, stainless steel gasket, metallic lithium, diaphragm (polypropylene microporous membrane Celgard2400), electrolyte (1MLiFP6, EC:EMC:DMC=1:1:1 (volume ratio), additives are LiDFOB and LiTFSI), positive electrode sheet, and positive electrode shell.
[0053] ③ Performance test: The battery charging and discharging performance, coulomb efficiency and cycle performance were tested using Wuhan Blue Electric CT2001A battery testing system. All batteries of the present invention were tested at 25°C and 1C.
[0054] In the above steps ① to ③, the reagents, materials, dosages, preparation and testing conditions are only one of the most preferred schemes, but the embodiments of the present invention are not limited thereto.
[0055] Table 2~Table 4 and Figure 3~Figure 11 The advantages of specific HNBR are demonstrated in three aspects: ACN content, hydrogen saturation and Mooney viscosity number.
[0056] Comparative Examples 1-3 and Examples 1-9 will be described in detail in conjunction with the above charts.
[0057] Comparative Example 1
[0058] Preparation and testing: PVDF and LFP materials are assembled into batteries to study their electrochemical properties. The specific process is as follows. ① Preparation of pole pieces: Take LFP, PVDF, and conductive carbon black in a mass ratio of 8:1:1, mix and grind in an appropriate amount of NMP solvent (the general NMP to HNBR feed ratio is 4mL:150mg. For a very small number of HNBRs that are difficult to dissolve, the amount of NMP can be increased appropriately, for example, 5mL:150mg, to ensure its dissolution) to obtain a uniform slurry. The slurry is evenly coated on carbon-coated aluminum foil with a coating thickness of 50 μm. After vacuum drying at 120°C for 12 h, it is cut into positive pole pieces with a diameter of 12 mm and placed in a glove box for use. ②Battery assembly: The prepared positive electrode sheet is assembled into a liquid button cell in the order of negative electrode shell, spring gasket, stainless steel gasket, metal lithium, Celgard2400 diaphragm, electrolyte (1M LiFP6, EC:EMC:DMC=1:1:1 (volume ratio), additives are LiTFSI+LiDFOB, the content of each is 0.5% of the concentration of LiFP6, totaling 1.0%), positive electrode sheet, and positive electrode shell in a glove box filled with argon (O2 and H2O content are both <0.1ppm). ③Performance test: The battery's charge and discharge performance, coulomb efficiency, and cycle performance are tested using the Wuhan Blue Electric CT2001A battery test system, with the test conditions being 25°C and 1C rate.
[0059] Performance description: The battery performance of comparative example 1 is shown in Table 2 and Figure 3 During the first cycle, the reversible capacity is 132 mAh g -1 , the coulombic efficiency is 97.23%, the charge-discharge voltage difference is 0.13 V; after 500 cycles, the capacity retention rate is 96.2%. Overall, the performance of PVDF-LFP battery is excellent, with high coulombic efficiency in the first week, small charge-discharge voltage difference, and good long-cycle performance, but the reversible capacity is low in the early stage.
[0060] Comparative Example 2
[0061] Preparation and testing: The only difference from Comparative Example 1 is that the active material in the electrode preparation process of ① is replaced from LFP to LCO.
[0062] Performance description: The battery performance of comparative example 2 is shown in Table 3 and Figure 6 During the first cycle, the reversible capacity is 137 mAh g -1 , the coulombic efficiency is 95.43%, the charge-discharge voltage difference is 0.07 V; after 300 cycles, the capacity retention rate is 99.0%. Overall, the performance of the PVDF-LCO battery is excellent, with high coulombic efficiency in the first week, extremely low charge-discharge voltage difference, and good long-cycle performance, but there is activation phenomenon in the first few weeks and the reversible capacity is low.
[0063] Comparative Example 3
[0064] Preparation and testing: The only difference from Comparative Example 1 is that the active material in the electrode preparation process of ① is replaced from LFP to NCM523.
[0065] Performance description: The battery performance of comparative example 3 is shown in Table 4 and Fig. 9 As shown: During the first cycle, the reversible capacity is 119 mAh g -1 , the coulombic efficiency is 82.0%, the charge-discharge voltage difference is 0.11 V; after 200 cycles, the capacity retention rate is 96.7%. Overall, the performance of the PVDF-NCM523 battery is excellent, the coulombic efficiency in the first week is low, the charge-discharge voltage difference is small, the long-cycle performance is good, but the initial reversible capacity is low.
[0066] Example 1
[0067] Preparation and testing: The only difference from Comparative Example 1 is that the binder in the preparation process of the electrode is replaced by HNBR from PVDF. The biggest difference between samples 1 to 4 is that they have different ACN contents. As shown in Table 1, the ACN contents of samples 1 to 4 are 26%-29%, 16%-20%, 33% and 41% respectively.
[0068] Performance comparison: The performance of all batteries in this example is as follows Figure 3 As shown in Table 2. It can be found that HNBR binders with different ACN contents have a significant effect on the battery. Sample 1 has the best battery performance, with a reversible capacity significantly higher than PVDF, and 500-week cycle stability and capacity retention rate comparable to or even better than PVDF. The initial capacity of the battery in Sample 2 is much higher than that of PVDF, but it decays faster. The initial capacity of Sample 3 is slightly lower than that of PVDF, but the capacity retention rate is comparable. Sample 4 is significantly weaker than Samples 1 to 3 and PVDF. This shows that the influence of HNBR binders with suitable ACN content on LFP electrodes or battery systems is crucial.
[0069] Example 2
[0070] Preparation and testing: The only difference from Comparative Example 1 is that the binder in the preparation process of the electrode is replaced by HNBR from PVDF. The biggest difference between samples 1 and 5-7 is that they have different hydrogen saturations. As shown in Table 1, the hydrogen saturations of samples 1 and 5-7 are >99%, 96%, 90%-92% and 91% respectively.
[0071] Performance comparison: The performance of all sample batteries in this example is as follows Figure 4As shown in Table 2. It can be found that when matched with LFP, the hydrogen saturation of HNBR has little effect on the battery performance. The evidence is that the hydrogen saturation of the three HNBR samples 1, 5, and 6 decreases in turn, but the reversible capacity and cycle performance of the battery do not change much. The performance of sample 7 is significantly lower, which may be due to the combined effect of lower hydrogen saturation (91%), higher ACN content (36.5, see the analysis of Example 1 for details) or Mooney viscosity (57.5, see the analysis of Example 3 for details).
[0072] Example 3
[0073] Preparation and testing: The only difference from Comparative Example 1 is that the binder in the preparation process of the electrode is replaced by HNBR from PVDF. The biggest difference between samples 1 and 8-10 is that they have different Mooney viscosity numbers. As shown in Table 1, the Mooney viscosity numbers of samples 1 and 8-10 are 40-45, 20-30, 60-70 and "-" (sample 10 is liquid HNBR, no Mooney viscosity number, molecular weight Mw is 20000-40000).
[0074] Performance comparison: The performance of all batteries in this example is as follows Figure 5 As shown in Table 2. It can be found that the Mooney viscosity has a great influence on the performance of HNBR binder in LFP battery. When the Mooney viscosity is low, HNBR (samples 1 and 8) show high specific capacity, capacity retention rate and cycle stability, and sample 1 is more stable. The Mooney viscosity number is related to the molecular chain length and distribution degree, which is related to the adhesion, dispersibility and mechanical strength of HNBR, thus affecting the performance of the electrode or battery. This shows that it is necessary to select HNBR with a suitable Mooney viscosity number for LFP batteries.
[0075] Table 2 Performance of all batteries in Examples 1-3 and Comparative Example 1
[0076]
[0077] Example 4
[0078] Preparation and testing: The only difference from Example 1 is that the active material in the electrode preparation process is replaced by LCO from LFP, and the effects of samples 1 to 4 with different ACN contents on the LCO battery performance are studied. The ACN contents of samples 1 to 4 are 26%-29%, 16%-20%, 33% and 41% respectively.
[0079] Performance comparison: The performance of all batteries in this example is as follows Figure 6As shown in Table 3. It can be found that HNBR binders with different ACN contents have a significant effect on the battery. Sample 1 has the best battery performance, with a reversible capacity significantly higher than PVDF, and 300-week cycle stability and capacity retention rate comparable to or even better than PVDF. Samples 2 and 3 have significantly lower initial capacities than PVDF, and their capacity retention rates are comparable to those of sample 1 and PVDF. Sample 4 is significantly weaker than samples 1 to 3 and PVDF. This shows that the influence of HNBR binders with suitable ACN content on LFP electrodes or battery systems is crucial.
[0080] Example 5
[0081] Preparation and testing: The only difference from Example 2 is that the active material in the electrode preparation process is replaced by LCO from LFP, and the effect of samples 1 and 5-7 with different hydrogen saturations on the performance of LCO batteries is studied. The hydrogen saturations of samples 1 and 5-7 are >99%, 96%, 90%-92% and 91%, respectively.
[0082] Performance comparison: The performance of all sample batteries in this example is as follows Figure 7 As shown in Table 3. It can be found that when matched with LCO, the hydrogen saturation of HNBR has a great influence on the battery performance. The battery performance of sample 1 is obviously the best, and the reversible capacity is significantly higher than that of sample 5 and PVDF. The 300-week cycle stability and capacity retention rate are comparable to or even better than those of PVDF. Samples 6 and 7 decay rapidly to zero after about 10 cycles. This is completely different from the situation of the LFP electrode in Example 2 (the effect of hydrogen saturation on the performance of the LFP battery is not significant). This shows that the high oxidation environment on the surface of LCO places higher requirements on the hydrogen saturation of HNBR. When matching LCO, having a high hydrogen saturation (preferably >99%) is a necessary condition for HNBR.
[0083] Example 6
[0084] Preparation and testing: The only difference from Example 3 is that the active material in the preparation process of the electrode ① is replaced by LCO from LFP, and the influence of samples 1 and 8 to 10 with different Mooney viscosity numbers on the performance of LCO batteries is studied. The Mooney viscosity numbers of samples 1 and 8 to 10 are 40-45, 20-30, 60-70 and "-" (sample 10 is liquid HNBR, no Mooney viscosity number, molecular weight Mw is 20000-40000).
[0085] Performance comparison: The performance of all batteries in this example is as follows Figure 8As shown in Table 3. Similar to LFP, the Mooney viscosity number has a great influence on the performance of HNBR in LCO: HNBR with low Mooney viscosity (samples 1 and 8) exhibits high specific capacity, capacity retention rate and cycle stability, sample 1 is more stable and has higher capacity; HNBR with higher Mooney viscosity (sample 9) has rapid performance decline. The difference is that sample 10 with ultra-high Mooney viscosity has better performance than sample 8. This shows that the high oxidation environment on the surface of LCO places higher requirements on the molecular structure and properties (adhesion, dispersibility and mechanical strength, etc.) of HNBR. When matching LCO, HNBR with a suitable Mooney viscosity number is necessary.
[0086] Table 3 Performance of all batteries in Examples 4-6 and Comparative Example 2
[0087]
[0088] Example 7
[0089] Preparation and testing: The only difference from Example 1 is that the active material in the electrode preparation process is replaced by NCM523 from LFP, and the effects of samples 1 to 4 with different ACN contents on the performance of NCM523 batteries are studied. The ACN contents of samples 1 to 4 are 26%-29%, 16%-20%, 33% and 41% respectively.
[0090] Performance comparison: The performance of all batteries in this example is as follows Fig. 9 As shown in Table 4. It can be found that HNBR binders with different ACN contents have a significant effect on the battery. Sample 1 has the best battery performance, with a higher reversible capacity than PVDF in the first 120 weeks, and both the cycle stability and capacity retention rate decreased in the later period. The initial capacity of samples 2 and 4 is significantly lower than that of PVDF, and the capacity of sample 3 in the first 20 weeks is the highest, but it also decreases fastest in the later period. This shows that the influence of HNBR binder with a suitable ACN content on the NCM523 electrode or battery system is crucial.
[0091] Example 8
[0092] Preparation and testing: The only difference from Example 2 is that the active material in the electrode preparation process is replaced by NCM523 from LFP, and the effect of samples 1 and 5-7 with different hydrogen saturations on the performance of NCM523 batteries is studied. The hydrogen saturations of samples 1 and 5-7 are >99%, 96%, 90%-92% and 91% respectively.
[0093] Performance comparison: The performance of all sample batteries in this example is as follows Fig.10As shown in Table 4. Similar to LCO, the hydrogen saturation of HNBR has a great influence on the performance of NCM523 batteries. Sample 1 has the best battery performance, and its reversible capacity, 200-week cycle stability and capacity retention are comparable to those of PVDF. Sample 5 is significantly weaker than sample 1 and PVDF, but significantly better than samples 6 and 7. The initial capacity of samples 6 and 7 is only 90-95 mAhg -1 , the capacity retention rate after 200 cycles is only 50%-55%. This is completely different from the situation of the LFP electrode in Example 2 (the hydrogen saturation has little effect on the performance of the LFP battery). This shows that the high oxidation environment on the surface of NCM523 places higher requirements on the hydrogen saturation of HNBR. When matching NCM523, having a high hydrogen saturation (preferably >99%) is a necessary condition for HNBR.
[0094] Example 9
[0095] Preparation and testing: The only difference from Example 3 is that the active material in the preparation process of the electrode ① is replaced by NCM523 from LFP, and the influence of samples 1 and 8 to 10 with different Mooney viscosity numbers on the performance of NCM523 batteries is studied. The Mooney viscosity numbers of samples 1 and 8 to 10 are 40-45, 20-30, 60-70 and "-" (sample 10 is liquid HNBR, no Mooney viscosity number, molecular weight Mw is 20000-40000).
[0096] Performance comparison: The performance of all batteries in this example is as follows Fig.11 and as shown in Table 4. Similar to LFP, the Mooney viscosity number has a great influence on the performance of HNBR in NCM523: HNBR with low Mooney viscosity (samples 1 and 8) exhibits high specific capacity, capacity retention rate and cycle stability, sample 1 is more stable and has higher capacity; sample 9 has lower capacity but good stability. The difference is that the performance of sample 10 with ultra-high Mooney viscosity increases from an initial capacity of 122 mAhg -1 The capacity retention rate of HNBR decreased rapidly, and after 200 cycles, it was only 52%. This shows that the high oxidation environment on the surface of NCM523 places higher demands on the molecular structure and performance (adhesion, dispersibility and mechanical strength, etc.) of HNBR. When matching NCM523, HNBR with a suitable Mooney viscosity number is necessary.
[0097] Table 4 Performance of all batteries in Examples 7-9 and Comparative Example 3
[0098]
[0099] Example 10
[0100] This example demonstrates the performance of Sample 1 in different electrolyte compositions (different solvents and lithium salts) and different electrolyte types (liquid and solid), and compares it with PVDF.
[0101] Preparation and testing: The battery preparation and testing steps differ from those of comparative example 1 only in the type and matching of the binder and electrolyte. The binders of this embodiment are sample 1 and PVDF; there are five types of electrolytes, namely EC+EMC+DMC+LiFP6+LiTFSI+LiDFOB (liquid), EC+EMC+DMC+LiFP6+LiTFSI (liquid), EC+DMC+FEC+LiFP6+LiTFSI (liquid), PVEC+APFB+LiTFSI+LiDFOB (solid), PEO+PFBBA+SN+LiTFSI (solid), the lithium salt concentration is 1M, and the additive concentration is 1.0% of the lithium salt concentration (when two additives are contained, their concentrations are each 0.5% of the lithium salt concentration, a total of 1.0%). The binders and different electrolytes are matched and assembled into batteries, a total of 10 battery combinations, see Table 5 for details.
[0102] Performance description: Table 5 shows the core parameters (first-week capacity, first-week coulombic efficiency, first-week charge-discharge voltage difference, and reversible capacity after long cycles) of sample 1 and PVDF described in this example in five electrolytes. Two main conclusions can be drawn. ① Whether sample 1 (HNBR) or PVDF is used as a binder, the performance of the battery will vary in different electrolyte systems. The reason is that the electrolyte components will affect the interfacial reaction kinetics and system stability of the positive and negative electrodes of the battery. ② In the same electrolyte system, the first-week capacity, voltage difference, and reversible capacity after 500 cycles of the sample 1 battery are significantly better than (or equivalent to) PVDF batteries, but the first-week coulombic efficiency is slightly lower than that of PVDF.
[0103] Table 5 Performance of all batteries in Example 10
[0104]
[0105] Combining Table 1-Table 4, Examples 1-9 and Figure 3-Figure 11 Analysis shows that LFP, LCO, and NCM523 have strict and different requirements for the ACN content, hydrogen saturation, and Mooney viscosity of HNBR, which need to be considered comprehensively. When matching LFP, LCO, and NCM523 as lithium-ion batteries with positive electrode materials, sample 1 is significantly better than samples 2-10 in terms of specific capacity, coulomb efficiency, charge and discharge voltage difference, cycle stability, and capacity retention rate. It can be determined that sample 1 has more suitable comprehensive indicators, and its core parameters are: ACN content 26%-29%, hydrogen saturation>99%, and Mooney viscosity number 40-45.
[0106] Comparative analysis of Comparative Examples 1-3 and Examples 1-9 shows that Sample 1 is on par with PVDF in terms of specific capacity, Coulomb efficiency, charge-discharge voltage difference, cycle stability, and capacity retention, and is even superior to PVDF in terms of specific capacity. This shows that the special HNBR of the present invention is feasible for use as a positive electrode material for lithium-ion batteries.
[0107] Combining Table 1-Table 4, Comparative Examples 1-3, Examples 1-9 and Figure 3-Figure 11 Analysis shows that the lithium-ion batteries assembled from sample 1 and active materials (LFP, LCO, NCM523) all show performance equal to or better than that of PVDF, indicating that the special HNBR proposed in the present invention has good applicability in the application of lithium-ion battery positive electrode materials.
[0108] From the analysis of Table 5, it can be seen that sample 1 (HNBR) has good compatibility with various electrolytes. In the same electrolyte system, the first-week capacity, voltage difference, and reversible capacity after 500 cycles of sample 1 battery are significantly better than (or equivalent to) PVDF batteries, but the first-week coulombic efficiency is slightly lower than that of PVDF.
[0109] The specific implementation contents described above are specific descriptions of the contents of the present invention in combination with preferred embodiments, but it cannot be determined that the specific implementation of the present invention is limited to the embodiments. For those skilled in the art who understand the field to which the present invention belongs, other evolutions and substitutions can be made without departing from the research ideas of the present invention, and these deductions and substitutions are all included in the scope defined by the claims of the present invention.
Claims
1. An application of HNBR as a positive electrode binder for lithium-ion batteries, characterized in that: The HNBR has a hydrogenation saturation of ≥90%, an ACN content of 26%-29%, and a Mooney viscosity ML (1+4) @ 100°C of 20-45.
2. The use according to claim 1, characterized in that: In the lithium-ion battery, the HNBR is used alone as a positive electrode binder.
3. The use according to claim 1 or 2, characterized in that: The hydrogenation saturation of the HNBR is ≥95%.
4. The use according to claim 3, characterized in that: The hydrogenation saturation of the HNBR is >99%.
5. The use according to claim 1 or 2, characterized in that: The Mooney viscosity ML (1+4) @ 100°C of the HNBR is 40-45.
6. The use according to claim 1 or 2, characterized in that: The ACN content of the HNBR is 26%-29%, the hydrogenation saturation is >99%, and the Mooney viscosity ML (1+4) @ 100°C is 40-45.
7. A positive electrode for a lithium-ion battery, obtained by uniformly coating a positive electrode slurry for a lithium-ion battery on a current collector and then drying the same; characterized in that: The positive electrode slurry of the lithium-ion battery comprises a positive electrode active material, a binder, a conductive agent and a solvent. The binder is HNBR, the hydrogenation saturation of the HNBR is ≥90%, the ACN content is 26%-29%, and the Mooney viscosity ML (1+4) @ 100°C is 20-45.
8. The lithium ion battery positive electrode as claimed in claim 7, characterized in that: The Mooney viscosity ML (1+4) @ 100°C of the HNBR is 40-45.
9. The lithium ion battery positive electrode as claimed in claim 8, characterized in that: The ACN content of the HNBR is 26%-29%, the hydrogenation saturation is >99%, and the Mooney viscosity ML (1+4) @ 100°C is 40-45.
10. A lithium ion battery, characterized in that: The positive electrode of the lithium ion battery is the positive electrode of the lithium ion battery according to any one of claims 7 to 9.
Citation Information
Patent Citations
Positive electrode active material pre-dispersion composition, positive electrode for secondary battery, and lithium secondary battery comprising same
CN109845005A
Positive electrode for lithium secondary battery having primer layer containing lithium iron phosphate
CN115244731A
Conductive material dispersion liquid, composition for secondary battery electrode using same, electrode film, and secondary battery
CN117157775A
Positive plate as well as preparation method and application thereof
CN118198367A
Anode for a lithium-ion battery cell, production method thereof and battery including same