Composite diaphragm and lithium ion battery

By designing a composite separator including base film, non-conductive particle coating and bonding layer in lithium-ion batteries, the ratio and surface density optimization of the particulate polymer and non-conductive particles is solved. The non-fluorine separator has a low bonding strength of the non-fluorine separator. Problem, a battery separator with high bond strength and breathability is achieved.

CN118970379AActive Publication Date: 2024-11-15SHENZHEN HAODYNE TECH CO LTD

Patent Information

Application Number
CN202411435485.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-15
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

The existing non-fluorine diaphragm adhesive has low adhesion strength, resulting in low bonding strength between the composite diaphragm and the electrode sheet, which poses a safety hazard.

Method used

Using a composite separator design including a base film, a non-conductive particle coating and a bonding layer, the bonding layer uses particulate polymers and non-conductive particles to ensure that the average particle size of the particulate polymer and non-conductive particles are at 0.4. Within the range of -100, the bonding layer density is between 0.1-0.6g/m2, which improves bonding strength and breathability.

Benefits of technology

The bonding strength and breathability between the composite diaphragm and the pole sheet are significantly improved, and the safety and performance of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a composite diaphragm and a lithium ion battery in order to solve the problem of low bonding strength between a composite diaphragm prepared by using a non-fluorine diaphragm binder and a pole piece due to low bonding force of the non-fluorine diaphragm binder in the prior art. The composite diaphragm comprises a base membrane, a non-conductive particle coating located on the surface of the base membrane, and a bonding layer located on the surface of the non-conductive particle coating, the adhesive layer comprises a diaphragm adhesive, the diaphragm adhesive comprises a granular polymer, and the average particle size D1 of the granular polymer is 0.2-6 [mu] m; the non-conductive particle coating comprises non-conductive particles, and the average particle size D2 of the non-conductive particles is 0.1-2 [mu] m; the average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles meet the condition that D1 / D2 is greater than or equal to 0.4. The composite diaphragm provided by the invention has excellent air permeability and bonding strength between the composite diaphragm and a pole piece at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a composite diaphragm and a lithium ion battery using the composite diaphragm. Background Art

[0002] Lithium-ion battery is a rechargeable battery with broad application prospects. It is favored by various industries because of its high energy density, long life, small size, maintenance-free and environmentally friendly characteristics. It has moved from the fields of mobile phones and laptops to electric bicycles, electric vehicles, energy storage and various portable devices. It is an ideal mobile power source.

[0003] Lithium-ion batteries are usually composed of a positive electrode, a negative electrode, a separator, an electrolyte, and a battery casing. The separator is one of the key internal components, and its function is to separate the positive and negative electrodes of the battery to prevent direct contact between the positive and negative electrodes and short circuit.

[0004] At present, the separators used in lithium-ion batteries are generally polyolefin porous membranes. Since this polyolefin porous membrane has a low melting point, when the battery temperature rises due to internal or external factors, the polyolefin porous membrane will shrink or melt, causing direct contact between the positive and negative electrodes, resulting in a battery short circuit, and then causing accidents such as battery combustion and explosion.

[0005] In order to solve these problems, inorganic particles are usually coated on the surface of the membrane substrate using a polymer adhesive to form a composite membrane. For example, ceramic particles are coated on the surface of the membrane substrate to form a ceramic / polymer composite membrane. It is hoped that the heat resistance of the ceramic particles can be used to reduce the thermal shrinkage of the membrane.

[0006] At the same time, a layer of diaphragm adhesive is coated on the surface of the ceramic coating to bond the diaphragm to the positive and negative electrodes, thereby fixing the battery structure.

[0007] At present, the most commonly used diaphragm adhesives on the market are mainly polyvinylidene fluoride (PVDF).

[0008] However, PVDF adhesives have problems such as scarce upstream fluorine resources, difficulty in recycling, and serious environmental pollution caused by decomposition products.

[0009] Therefore, it is an industry development trend to use non-fluorine diaphragm adhesives to achieve bonding between diaphragms and pole pieces.

[0010] However, the existing non-fluorine-based diaphragm adhesives (such as polyacrylate adhesives) have low bonding strength, and the composite diaphragm prepared using the diaphragm adhesive has the problem of low bonding strength between the diaphragm and the electrode. Summary of the invention

[0011] The technical problem to be solved by the present invention is that the existing non-fluorine diaphragm adhesive has low bonding strength, and the composite diaphragm prepared using the diaphragm adhesive has the problem of low bonding strength between the electrode and the electrode. The present invention provides a composite diaphragm and a lithium-ion battery.

[0012] In order to solve the above technical problems, the present invention provides a composite diaphragm, comprising a base film, a non-conductive particle coating located on the surface of the base film, and a bonding layer located on the surface of the non-conductive particle coating; The bonding layer includes a diaphragm binder, the diaphragm binder includes a granular polymer, and the average particle size D1 of the granular polymer is 0.2-6 μm; The non-conductive particle coating comprises non-conductive particles, and the average particle size D2 of the non-conductive particles is 0.1-2 μm; The average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles satisfy: D1 / D2≥0.4.

[0013] Preferably, the average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles satisfy: 0.4≤D1 / D2≤100.

[0014] Preferably, the glass transition temperature Tg of the granular polymer is 10-90°C.

[0015] Preferably, the granular polymer is a polymer comprising at least one of vinyl monomer units, (meth)acrylate monomer units, maleate monomer units, itaconate monomer units, maleimide monomer units, and (meth)acrylamide monomer units.

[0016] Preferably, the vinyl monomer unit is selected from at least one of aliphatic vinyl hydrocarbon compound units, alicyclic vinyl hydrocarbon compound units, aromatic vinyl hydrocarbon compound units, olefinic and propyl compound units, and vinyl compound units containing heteroatoms; The (meth)acrylic acid ester monomer unit is at least one selected from methacrylic acid ester monomer units and acrylic acid ester monomer units.

[0017] The maleate monomer unit includes at least one of C1-C12 monoalkyl maleate or C1-C12 dialkyl maleate; The itaconate monomer unit includes at least one of itaconate C1-C12 monoester and itaconate C1-C12 diester; The maleimide monomer unit includes at least one of a maleimide monomer unit, a C1-C12 alkyl-substituted maleimide monomer unit, and a C6-C16 aryl-substituted maleimide monomer unit; The (meth)acrylamide monomer units include at least one of (meth)acrylamide monomer units, N-methyl(meth)acrylamide monomer units, N-butylacrylamide monomer units, acetylacetonatoacrylamide monomer units, N-hydroxymethyl(meth)acrylamide monomer units, N,N'-methylenebis[(meth)acrylamide] monomer units, cinnamamide monomer units, N,N-dimethylacrylamide monomer units, N,N-dibenzylacrylamide monomer units, methacryloylformamide monomer units, N-methyl N-vinylacetamide monomer units, and N-vinylpyrrolidone monomer units.

[0018] Preferably, the thickness of the non-conductive particle coating is 0.5-4 μm.

[0019] Preferably, the surface density of the adhesive layer is 0.1-0.6 g / m 2 .

[0020] Preferably, the non-conductive particle coating comprises non-conductive particles, a ceramic binder, and a selectively added rheology modifier, a dispersant, and a wetting agent; In the non-conductive particle coating, the weight ratio of the non-conductive particles, the ceramic binder, the sodium carboxymethyl cellulose, the dispersant and the wetting agent is (88-96.3): (3-15): (0-3): (0-2): (0-2).

[0021] Preferably, the base film is selected from at least one of a polyethylene base film, a polypropylene base film, a polypropylene-polyethylene-polypropylene laminated base film or a non-woven fabric base film; And / or, the base film has a thickness of 3-12 μm.

[0022] In a second aspect, the present application provides a lithium-ion battery, comprising the composite separator as described above.

[0023] Through extensive research, the applicant discovered that the granular polymer in the bonding layer formed on the surface of the non-conductive particle coating is extremely easy to embed into the gaps between the non-conductive particles in the non-conductive particle coating. During the subsequent hot pressing process of the composite diaphragm and the electrode, the granular polymer in the bonding layer and the electrode are prone to insufficient contact, resulting in low bonding strength between the composite diaphragm and the electrode.

[0024] In view of the above research, the applicant set the bonding layer of the composite diaphragm to 0.1-0.6g / m 2 Within the range, a granular polymer having an average particle size D1 of 0.4-3 μm and a non-conductive particle having an average particle size D2 of 0.1-2 μm are used in combination, and D1 / D2 is defined as ≥ 0.4, so that the composite diaphragm has both excellent air permeability and bonding strength with the pole piece. DETAILED DESCRIPTION

[0025] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.

[0026] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0027] In the description of the present invention, the term "monomer unit" refers to a corresponding unit of a monomer structure formed on a polymer chain segment after a certain monomer participates in polymerization.

[0028] The term "average particle size" refers to the volume average particle size D of the particles. V 50.

[0029] The composite diaphragm provided by the present invention comprises a base film, a non-conductive particle coating located on the surface of the base film, and a bonding layer located on the surface of the non-conductive particle coating; The bonding layer includes a diaphragm binder, the diaphragm binder includes a granular polymer, and the average particle size D1 of the granular polymer is 0.4-3 μm; The non-conductive particle coating comprises non-conductive particles, and the average particle size D2 of the non-conductive particles is 0.1-2 μm; The average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles satisfy: D1 / D2≥0.4.

[0030] According to the present invention, in the bonding layer, the average particle size D1 of the granular polymer is 0.2-6μm. Specifically, the average particle size D1 of the granular polymer can be 0.1μm, 0.5μm, 0.8μm, 1μm, 1.2μm, 1.5μm, 1.8μm, 2μm, 2.1μm, 2.4μm, 2.5μm, 2.8μm, 3μm, 4μm, 5μm, or 6μm.

[0031] Preferably, the average particle size D1 of the granular polymer is 0.2-5 μm.

[0032] In the composite diaphragm provided by the present invention, if the average particle size D1 of the granular polymer is greater than 6 μm or less than 0.1 μm, the bonding strength between the composite diaphragm and the pole piece will be significantly reduced.

[0033] The reason may be that if D1 is greater than 6 μm, the granular polymer is easily fallen off after being formed on the surface of the non-conductive particle coating, resulting in a decrease in bonding strength; if D1 is less than 0.1 μm, the granular polymer is more easily embedded in the non-conductive particle coating, resulting in a decrease in bonding strength.

[0034] At the same time, for the composite diaphragm provided by the present invention, the surface density of the adhesive layer on its surface is 0.1-0.6 g / m 2 .

[0035] Specifically, the surface density of the adhesive layer can be 0.1 g / m 2 , 0.2g / m 2 , 0.3g / m 2 , 0.4g / m 2 , 0.5g / m 2 , 0.6g / m 2 .

[0036] Preferably, the surface density of the adhesive layer is 0.1-0.3 g / m 2 .

[0037] In the present invention, if the surface density of the bonding layer is not within the above range, the air permeability of the composite diaphragm will be reduced or the bonding strength between the composite diaphragm and the electrode sheet will be insufficient.

[0038] According to the present invention, the glass transition temperature of the granular polymer can vary within a wide range. Preferably, the glass transition temperature Tg of the granular polymer is 10-90°C.

[0039] More preferably, the temperature is 20-80°C.

[0040] The granular polymer in the present invention can adopt the existing non-fluorine adhesive used for bonding the separator and the pole piece, such as a polyacrylate adhesive, and the preparation method of the adhesive is known to those skilled in the art.

[0041] In the present invention, preferably, the particulate polymer is a polymer including at least one of vinyl monomer units, (meth)acrylate monomer units, maleate monomer units, itaconate monomer units, maleimide monomer units, and (meth)acrylamide monomer units.

[0042] Furthermore, the vinyl monomer unit is selected from at least one of aliphatic vinyl hydrocarbon compound units, alicyclic vinyl hydrocarbon compound units, aromatic vinyl hydrocarbon compound units, allyl compound units, and vinyl compound units containing heteroatoms.

[0043] Among them, the aliphatic vinyl hydrocarbon compounds include but are not limited to chain alkenes with 2-12 carbon atoms (exemplarily including but not limited to: ethylene, propylene, butene, isobutylene, pentene, heptene, diisobutylene, octene, dodecene, octadecene), α-olefins with 3-24 carbon atoms, and dienes with 4-12 carbon atoms (exemplarily including but not limited to: butadiene, isoprene, 1,4-pentadiene, 1,6-hexadiene and 1,7-octadiene).

[0044] The alicyclic vinyl hydrocarbon compounds include, but are not limited to, monocyclic or bicyclic olefins having 6-15 carbon atoms (exemplarily including, but not limited to, cyclohexene, vinylcyclohexene and ethylidene bicycloheptene), monocyclic or bicyclic dienes having 5-12 carbon atoms (exemplarily including, but not limited to, cyclopentadiene, cycloheptadiene, dicyclopentadiene, dicycloheptadiene), and terpene compounds (exemplarily including, but not limited to, limonene and indene).

[0045] The aromatic vinyl hydrocarbon compounds include but are not limited to styrene and substituted styrenes. The substituted styrenes illustratively include but are not limited to: α-methylstyrene, vinyltoluene, 2,4-dimethylstyrene, ethylstyrene, isopropylstyrene, butylstyrene, phenylstyrene, cyclohexylstyrene, benzylstyrene, crotonylstyrene, divinylbenzene, divinyltoluene, divinylxylene, trivinylbenzene, vinylnaphthalene, and p-tert-butylstyrene.

[0046] Vinyl compounds containing heteroatoms include, but are not limited to, vinyl (thio) ether, vinyl sulfone, acrylonitrile, methacrylonitrile, cyanostyrene, 4-vinylpyridine, 2-vinylpyridine, vinylimidazole, N-vinylpyrrole, and N-vinylthiopyrrolidone.

[0047] The (meth)acrylic acid ester monomer unit is at least one selected from methacrylic acid ester monomer units and acrylic acid ester monomer units.

[0048] The (meth)acrylate monomers illustratively include, but are not limited to, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, n-hexyl acrylate, n-octyl acrylate, isooctyl acrylate, isobornyl acrylate, phenoxyethyl acrylate, dicyclopentenyl acrylate, cyclohexyl acrylate, benzyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, carboxyethyl acrylate, methyl methacrylate, methyl ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-hexyl methacrylate, isooctyl methacrylate, isobornyl methacrylate, phenoxyethyl methacrylate, dicyclopentenyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, polyethylene glycol mono[(meth)acrylate] ester, (meth) aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, tert-butylaminoethyl methacrylate, glycidyl (meth)acrylate, tetrahydrofuran (meth)acrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, ethoxylated ethylene glycol diacrylate, ethoxylated ethylene glycol dimethacrylate, allyl methacrylate, diallyl phthalate, diallyl adipate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol diacrylate At least one of ester, pentaerythritol dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, aminoethyl acrylate, aminoethyl methacrylate, dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl acrylate, diethylaminoethyl methacrylate, and tert-butylaminoethyl methacrylate.

[0049] The maleate monomer unit includes at least one of C1-C12 monoalkyl maleate or C1-C12 dialkyl maleate.

[0050] As known to those skilled in the art, the above C1-C12 means that the number of carbon atoms is 1-12.

[0051] Specifically, the maleate monomer may include at least one of monomethyl maleate, dimethyl maleate, monoethyl maleate, diethyl maleate, monopropyl maleate, dipropyl maleate, monobutyl maleate, dibutyl maleate, monooctyl maleate, and dioctyl maleate.

[0052] The itaconate ester monomer unit includes at least one of itaconate C1-C12 monoester and itaconate C1-C12 diester.

[0053] Specifically, the itaconate ester monomer may include at least one of monomethyl itaconate, dimethyl itaconate, monoethyl itaconate, diethyl itaconate, monobutyl itaconate, dibutyl itaconate, monooctyl itaconate, and dioctyl itaconate.

[0054] The maleimide monomer unit includes at least one of maleimide, C1-C12 alkyl-substituted maleimide, and C6-C16 aryl-substituted maleimide.

[0055] The (meth)acrylamide monomer units include at least one of (meth)acrylamide monomer units, N-methyl(meth)acrylamide monomer units, N-butylacrylamide monomer units, acetylacetonatoacrylamide monomer units, N-hydroxymethyl(meth)acrylamide monomer units, N,N'-methylenebis[(meth)acrylamide] monomer units, cinnamamide monomer units, N,N-dimethylacrylamide monomer units, N,N-dibenzylacrylamide monomer units, methacryloylformamide monomer units, N-methyl N-vinylacetamide monomer units, and N-vinylpyrrolidone monomer units.

[0056] In the present invention, the preparation method of the granular polymer is not particularly limited and can be any one of emulsion polymerization, suspension polymerization, dispersion polymerization, and precipitation polymerization, as long as the particle size and glass transition temperature of the prepared granular polymer meet the particle size range.

[0057] The granular polymer in the present invention can also be obtained commercially by selecting a granular polymer product having a desired average particle size D1 and glass transition temperature.

[0058] According to the present invention, the bonding layer in the composite separator is formed of a separator binder containing the above-mentioned particulate polymer.

[0059] The method for forming the above-mentioned bonding layer can adopt the existing method, for example, the membrane bonding agent is coated on the non-conductive particle coating through a conventional coating process.

[0060] It should be noted that, as mentioned above, the surface density of the adhesive layer formed by coating must be between 0.1-0.6 g / m 2 within the range.

[0061] In the present invention, the non-conductive particle coating comprises non-conductive particles, a ceramic binder, and a selectively added rheology modifier, a dispersant, and a wetting agent.

[0062] The rheology modifier may include at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium polyacrylate, and lithium polyacrylate.

[0063] Among them, non-conductive particles are well known to those skilled in the art. Specifically, the non-conductive particles are non-conductive, insoluble in water used as a dispersion medium in the slurry and a non-aqueous electrolyte used in a secondary battery, and can maintain their shape.

[0064] Furthermore, since the non-conductive particles are electrochemically stable, they exist stably in the separator under the use environment of the secondary battery.

[0065] As the non-conductive particles, for example, various inorganic particles and heat-resistant organic particles can be used.

[0066] As inorganic particles, there can be cited, for example, oxide particles such as hydrated aluminum oxide, aluminum oxide, boehmite, silicon dioxide, titanium dioxide, zirconium dioxide, calcium oxide, magnesium oxide, magnesium hydroxide, and aluminum oxide-silicon dioxide composite oxides; nitride particles such as aluminum nitride and boron nitride; covalently bonded crystal particles such as silicon and diamond; sparingly soluble ionic crystal particles such as calcium carbonate, barium titanate, barium sulfate, calcium fluoride, and barium fluoride; and clay particles such as talc and montmorillonite.

[0067] Examples of heat-resistant organic particles include polyethylene, polystyrene, polydivinylbenzene, crosslinked styrene-divinylbenzene copolymers, various crosslinked polymer particles such as polyimide, polyamide, polyamideimide, melamine resin, phenolic resin, benzoguanamine-formaldehyde condensate, and heat-resistant polymer particles such as polysulfone, polyacrylonitrile, polyaramid, polyacetal, and thermoplastic polyimide.

[0068] Here, the heat-resistant organic particles are different from the above-mentioned particulate polymer in that the particulate polymer has a binding ability, while the heat-resistant organic particles do not have a binding ability.

[0069] In the present invention, the non-conductive particles are preferably inorganic particles, and more preferably boehmite, hydrated alumina, and aluminum oxide.

[0070] According to the present invention, the average particle size D2 of the non-conductive particles is 0.1-2 μm.

[0071] Specifically, the average particle size D2 of the non-conductive particles may be 0.1 μm, 0.2 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, or 2 μm.

[0072] Preferably, the average particle size D2 of the non-conductive particles is 0.2-1.5 μm.

[0073] In the composite diaphragm provided by the present invention, if the average particle size D2 of the non-conductive particles is greater than 2 μm, it is not conducive to balancing the heat resistance of the composite diaphragm and the volume energy density of the battery.

[0074] If the average particle size D2 of the non-conductive particles is less than 0.1 μm, the air permeability of the composite diaphragm will increase too much, the air permeability will decrease, the internal resistance of the battery will be too high, and the performance of the prepared battery will be poor.

[0075] Importantly, in the present invention, the average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles satisfy: D1 / D2≥0.4.

[0076] The applicant of the present invention has creatively used the above-mentioned granular polymer with a specific average particle size and non-conductive particles through extensive research, and maintained the surface density of the adhesive layer at 0.1-0.6 g / m 2 Within this range, the granular polymer in the bonding layer formed on the surface of the non-conductive particle coating can be effectively inhibited from embedding into the gaps between the non-conductive particles in the non-conductive particle coating, thereby ensuring that in the subsequent hot pressing process of the composite diaphragm and the electrode piece, the granular polymer in the bonding layer and the electrode piece are in full contact, thereby improving the bonding strength between the composite diaphragm and the electrode piece.

[0077] In addition, the composite membrane also has excellent air permeability.

[0078] Preferably, the average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles satisfy: 0.4≤D1 / D2≤100, more preferably 0.6≤D1 / D2≤60.

[0079] According to the present invention, the thickness of the non-conductive particle coating is 0.5-4 μm.

[0080] Preferably it is 0.5-3 μm.

[0081] When the thickness of the non-conductive particle coating is less than 0.5 μm, the heat resistance of the composite separator will decrease, and the prepared battery will have a greater safety risk.

[0082] When the thickness of the non-conductive particle coating is greater than 4 μm, the composite separator will be too thick and the energy density of the prepared battery will be low.

[0083] The ceramic binder in the non-conductive particle coating serves to bond the non-conductive particles to the base film.

[0084] The ceramic binder in the present invention can be any of the existing ceramic binders, and ceramic binders with the required particle size and glass transition temperature can be directly purchased from the market.

[0085] The wetting agent may be any of various existing wetting agents, for example, any one or a mixture of several of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether and polyether-modified polysiloxane.

[0086] The dispersant may be any of the existing dispersants, for example, sodium polyacrylate.

[0087] In the present invention, in the non-conductive particle coating, the weight ratio of the non-conductive particles, the ceramic binder, the rheology modifier, the dispersant, and the wetting agent is (88-96.3): (3-15): (0-3): (0-2): (0-2).

[0088] In the present invention, the above weight ratio refers to the weight ratio between the substances, not the percentage.

[0089] Preferably, in the non-conductive particle coating, the weight ratio of the non-conductive particles, the ceramic binder, the rheology modifier, the dispersant, and the wetting agent is (88-96.3): (3-15): (0.5-3): (0.1-2): (0.1-2).

[0090] As known to those skilled in the art, the non-conductive particle coating is prepared from a non-conductive particle slurry.

[0091] For example, the non-conductive particle slurry is coated on the base film and dried in an oven.

[0092] The present invention does not particularly limit the base film, and the base film can be a polymer membrane commonly used in the art. For example, the base film can be selected from a polyethylene base film, a polypropylene base film, a polypropylene-polyethylene composite base film or a non-woven fabric base film, wherein the polypropylene-polyethylene composite base film refers to a base film formed by laminating polypropylene and polyethylene. The present invention does not limit the stacking order and number of layers of polypropylene and polyethylene, and can be a polypropylene-polyethylene double-layer base film, a polypropylene-polyethylene-polypropylene three-layer base film, or a polypropylene-polyethylene-polyethylene-polypropylene four-layer base film.

[0093] Preferably, the base film is selected from at least one of a polyethylene base film, a polypropylene base film, a polypropylene-polyethylene-polypropylene laminated base film or a non-woven fabric base film.

[0094] The thickness of the base film can vary within a wide range. Preferably, the thickness of the base film is 3-12 μm.

[0095] In a second aspect, the present application provides a lithium-ion battery, comprising the composite separator as described above.

[0096] The composite diaphragm provided by the present invention has excellent air permeability and bonding strength with the pole piece.

[0097] The present invention is further described below by way of examples.

[0098] Example 1 The battery of this embodiment is prepared by a method comprising the following steps: 1) Diaphragm adhesive Use SL814 from Shenzhen Haodian Technology Co., Ltd.

[0099] 2) Preparation of diaphragm A non-conductive particle slurry was prepared with 93.4 parts of non-conductive boehmite powder, 6 parts of ceramic binder (SWA610 from Shenzhen Haodian Technology Co., Ltd.), 0.3 parts of dispersant sodium polyacrylate, 1 part of sodium carboxymethyl cellulose, and 0.3 parts of wetting agent alkylphenol polyoxyethylene ether. The non-conductive particle slurry was coated on one surface of a polyethylene base film with a thickness of 9 μm. After drying in an oven at 50°C, a non-conductive particle coating was formed on the surface of the base film.

[0100] The membrane adhesive of step 1) is coated on the surface of the non-conductive particle coating, and the adhesive layer is obtained after drying.

[0101] Specific parameters of the granular polymer, adhesive layer, non-conductive particles, non-conductive particle coating and base film are shown in Table 1.

[0102] 3) Preparation of positive electrode N-methylpyrrolidone is used to disperse positive electrode active particles of lithium nickel cobalt manganese oxide NCM523, conductive carbon black Super P and binder polyvinylidene fluoride to form a positive electrode slurry; the positive electrode slurry is evenly coated on Al foil by coating, and after baking and rolling processes, a positive electrode including a positive electrode active layer is obtained; Among them, the mass ratio of positive electrode active particles, conductive agent and binder is 97.5:1.0:1.5.

[0103] 4) Preparation of negative electrode Deionized water is used to disperse negative electrode active particles artificial graphite, conductive carbon black Super P, a binder of sodium carboxymethyl cellulose and styrene-butadiene latex to form a negative electrode slurry; then a negative electrode active layer is formed on the surface of the negative electrode current collector by coating, baking and rolling processes to obtain a negative electrode; Among them, the mass ratio of negative electrode active particles, conductive agent and binder (the mass ratio of sodium carboxymethyl cellulose to styrene butadiene latex is 1:1.5) is 96.5:1.0:2.5.

[0104] 5) Battery preparation The prepared positive electrode, the composite separator and the negative electrode are stacked in sequence, and then wound to obtain a battery cell, the battery cell is placed in an aluminum-plastic film, an electrolyte is injected into the bare battery cell, and a battery is obtained through vacuum packaging, standing, formation, shaping and capacity testing. The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, ethyl methyl carbonate and diethyl carbonate, wherein the ratio of ethylene carbonate: ethyl methyl carbonate: diethyl carbonate is 3:2:5, and the concentration of lithium hexafluorophosphate is 1 mol / L.

[0105] Examples 2-7, Comparative Examples 1-6 A composite separator and a battery are prepared according to the method of Example 1, except that the parameters of the granular polymer, the adhesive layer, the non-conductive particles and the non-conductive particle coating are adjusted according to the contents of Table 1 (wherein, granular polymers and non-conductive particles of different particle sizes are purchased as shown in Table 1).

[0106] Table 1

[0107] Performance Testing The following performance tests were performed on the composite diaphragms in the examples and comparative examples, and the results are shown in Table 2; 1. Diaphragm air permeability value-added test Refer to the air permeability test in GB / T 36363-2018 "Polyolefin separators for lithium-ion batteries": Cut three pieces of diaphragm from the film roll at an interval of 150 mm in the longitudinal direction. If the diaphragm width is ≥100 mm, the sample size is 100 mm × 100 mm. If the diaphragm width is <100 mm, the sample size is 100 mm × diaphragm width.

[0108] Place the diaphragm in the test head of a permeability meter suitable for the test range to test the permeability time. Take the average value of 3 test results as the permeability time of the diaphragm, in units of s / 100cc.

[0109] The membrane permeability increment is the difference between the permeability time of the membrane coated with non-conductive particles and adhesive and the permeability time of the membrane with polyolefin base film, and the unit is s / 100cc.

[0110] 2. Peel strength test The composite diaphragm and the positive electrode sheet prepared by the scheme of the present invention were cut into strips of 20 mm*100 mm respectively, cold pressed for 60 seconds at 95°C and 2 MPa, and subjected to a 180° peel strength test using an electronic tensile testing machine. The test results were taken as the average value of the three samples.

[0111] Table 2

[0112] It can be seen from the test results in Table 2 that the composite diaphragm provided by the present invention can effectively improve air permeability and bonding strength.

[0113] When the average particle size D1 of the granular polymer, the surface density of the adhesive layer, the average particle size D2 of the non-conductive particles, and the ratio D1 / D2 are not within the range disclosed in the present invention, the air permeability and adhesive strength of the composite membrane are reduced to varying degrees.

[0114] Specifically, by comparing the test results of Examples 1-7 with Comparative Example 1, it can be seen that if the ratio of D1 / D2 is too small, the peel strength between the composite diaphragm and the electrode sheet will be significantly reduced, and its air permeability will also be reduced to a certain extent.

[0115] By comparing the test results of Examples 1-7 with Comparative Examples 2 and 3, it can be seen that under the scheme of the present invention, if the average particle size D1 of the granular polymer is too small, the air permeability value of the composite diaphragm will increase significantly and the air permeability will decrease significantly.

[0116] If the average particle size D1 of the granular polymer is too large, the peel strength between the composite diaphragm and the electrode will be significantly reduced.

[0117] By comparing the test results of Examples 1-7 with Comparative Example 4, it can be seen that under the scheme of the present invention, if the average particle size D2 of the non-conductive particles is too small, the air permeability value of the composite diaphragm will increase significantly and the air permeability will decrease significantly.

[0118] By comparing the test results of Examples 1-7 with Comparative Examples 5 and 6, it can be seen that if the surface density of the adhesive layer is too small, the peel strength between the composite diaphragm and the electrode will be significantly reduced; if the surface density of the adhesive layer is too large, the air permeability value of the composite diaphragm will be significantly increased and the air permeability will be significantly reduced.

[0119] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite diaphragm, It is characterized in that It includes a base film, a non-conductive particle coating located on the surface of the base film, and a bonding layer located on the surface of the non-conductive particle coating; The bonding layer includes a diaphragm binder, the diaphragm binder includes a granular polymer, and the average particle size D1 of the granular polymer is 0.2-6 μm; The non-conductive particle coating comprises non-conductive particles, and the average particle size D2 of the non-conductive particles is 0.1-2 μm; The average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles satisfy: D1 / D2≥0.

4.

2. The composite diaphragm according to claim 1, It is characterized in that The average particle size D1 of the granular polymer and the average particle size D2 of the non-conductive particles satisfy: 0.4≤D1 / D2≤100.

3. The composite diaphragm according to claim 1, It is characterized in that The glass transition temperature Tg of the granular polymer is 10-90°C.

4. The composite diaphragm according to any one of claims 1 to 3, It is characterized in that The granular polymer is a polymer including at least one of vinyl monomer units, (meth)acrylate monomer units, maleate monomer units, itaconate monomer units, maleimide monomer units, and (meth)acrylamide monomer units.

5. The composite diaphragm according to claim 4, It is characterized in that The vinyl monomer unit is selected from at least one of aliphatic vinyl hydrocarbon compound units, alicyclic vinyl hydrocarbon compound units, aromatic vinyl hydrocarbon compound units, allyl compound units, and vinyl compound units containing heteroatoms; The (meth)acrylate monomer unit is selected from at least one of a methacrylate monomer unit and an acrylate monomer unit; The maleate monomer unit includes at least one of C1-C12 monoalkyl maleate or C1-C12 dialkyl maleate; The itaconate monomer unit includes at least one of itaconate C1-C12 monoester and itaconate C1-C12 diester; The maleimide monomer unit includes at least one of a maleimide monomer unit, a C1-C12 alkyl-substituted maleimide monomer unit, and a C6-C16 aryl-substituted maleimide monomer unit; The (meth)acrylamide monomer units include at least one of (meth)acrylamide monomer units, N-methyl(meth)acrylamide monomer units, N-butylacrylamide monomer units, acetylacetonatoacrylamide monomer units, N-hydroxymethyl(meth)acrylamide monomer units, N,N'-methylenebis[(meth)acrylamide] monomer units, cinnamamide monomer units, N,N-dimethylacrylamide monomer units, N,N-dibenzylacrylamide monomer units, methacryloylformamide monomer units, N-methyl N-vinylacetamide monomer units, and N-vinylpyrrolidone monomer units.

6. The composite diaphragm according to claim 1, It is characterized in that The thickness of the non-conductive particle coating is 0.5-4 μm.

7. The composite diaphragm according to claim 1, It is characterized in that The surface density of the bonding layer is 0.1-0.6 g / m 2 .

8. The composite diaphragm according to any one of claims 1, 6 and 7, It is characterized in that The non-conductive particle coating comprises non-conductive particles, a ceramic binder, and a selectively added rheology modifier, a dispersant, and a wetting agent; In the non-conductive particle coating, the weight ratio of the non-conductive particles, the ceramic binder, the rheology modifier, the dispersant, and the wetting agent is (88-96.3): (3-15): (0-3): (0-2): (0-2).

9. The composite diaphragm according to claim 1, It is characterized in that The base film is selected from at least one of a polyethylene base film, a polypropylene base film, a polypropylene-polyethylene-polypropylene laminated base film or a non-woven fabric base film; And / or, the base film has a thickness of 3-12 μm.

10. A lithium ion battery, It is characterized in that The composite diaphragm comprises the composite diaphragm according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing ceramic composite diaphragm having high-adhesive polymer coating film

    CN110444718A

  • Battery diaphragm and battery

    CN115275524A

  • Twill polymer composite diaphragm as well as preparation method and application thereof

    CN115498360A

Cited By

  • Composite separator and lithium-ion battery

    WO2026082000A1