Method for removing coating layer and device for removing coating layer
By heating and extending in the laminated film and removing the coating using scrapers, wire brushes, sandblasting or water vapor, the problem of insufficient embrittlement of the coating film in high temperature environment is solved, and efficient removal and foundation of the laminated film is achieved The winding of material film is suitable for the manufacturing of ceramic green sheets and other fields.
Patent Information
- Application Number
- CN202380030633.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, when removing the plastic component coating film under high temperature environment, there is a problem that insufficient embrittlement makes it difficult to completely remove the coating film.
A laminated film composed of a substrate film and coating is used to transport and heat the coating through roll-to-roll. After cracks occur, the coating is removed using a scraper, wire brush, sandblasting or water vapor to ensure complete removal.
It realizes efficient and reliable removal of coating in the laminated film, avoids the problem of insufficient brittleness, and is suitable for the field of ceramic green sheet manufacturing and other fields.
Smart Images

Figure CN118973781A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a coating removal method and a coating removal device. Background Art
[0002] In recent years, from the perspective of protecting global resources and the environment, there has been an increasing trend in various fields to build a recycling-oriented society by reducing the generation of waste and making efforts to reuse and recycle it.
[0003] For example, Patent Document 1 discloses a method for treating a coated plastic part, characterized in that the coated plastic part having a coating film formed on the surface of the plastic part is exposed to a high temperature environment of 400° C. to 1000° C., and the coating film is embrittled and removed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: (Japanese) Patent Publication No. 2012-167213 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] However, the treatment method described in Patent Document 1 directly exposes plastic parts of various sizes to a high temperature environment, thereby embrittles the surface coating film. This may cause insufficient embrittlement of the coating film and may make it difficult to easily remove the coating film.
[0009] An object of the present invention is to provide a coating layer removal method and coating layer removal apparatus capable of easily removing the coating layer from a laminated film having a base film and a coating layer which is transported in a roll-to-roll manner.
[0010] Technical solutions for solving technical problems
[0011] [1] A method for removing a coating, comprising:
[0012] A step of preparing a roll formed by winding a laminated film having a base film and a coating layer;
[0013] a step of feeding the laminated film from the roll;
[0014] A step of stretching the laminated film after it is sent out;
[0015] A step of removing the coating layer from the stretched laminated film;
[0016] A step of winding the base film after the coating layer is removed into a roll.
[0017] [2] The method for removing a coating according to [1], wherein:
[0018] The step of removing the coating layer is a step of transferring the coating layer from the base film to the adhesive roll.
[0019] [3] The method for removing a coating according to [1], wherein:
[0020] The step of removing the coating layer is a step of scraping the coating layer off the base film using a scraper or a wire brush.
[0021] [4] The method for removing a coating according to [1], wherein:
[0022] The step of removing the coating layer is a step of scraping the coating layer off the base film using a sandblasting material.
[0023] [5] The method for removing a coating according to any one of [1] to [4], wherein:
[0024] The step of stretching the laminated film is performed while heating the laminated film.
[0025] [6] The method for removing a coating according to any one of [1] to [5], wherein:
[0026] After the step of stretching the laminated film and before the step of removing the coating layer, there is a step of blowing superheated water vapor toward the coating layer of the stretched laminated film.
[0027] [7] The method for removing a coating according to any one of [1] to [6],
[0028] The laminated film is used for manufacturing a ceramic green sheet and is the laminated film after the ceramic green sheet is peeled off.
[0029] [8] A coating removal device for removing a coating from a laminated film having a substrate film and a coating, wherein the coating removal device comprises:
[0030] a feeding mechanism for feeding the laminated film from a roll formed by winding the laminated film;
[0031] A stretching mechanism, which stretches the laminated film after being sent out;
[0032] a removing mechanism for removing the coating from the stretched laminated film;
[0033] A winding mechanism winds up the base film into a roll.
[0034] [9] The coating removal device according to [8], wherein:
[0035] The removal mechanism is a mechanism including an adhesive roll and transferring the coating layer from the base film to the adhesive roll.
[0036]
[10] The coating removal device according to [8], wherein:
[0037] The removal mechanism is a mechanism that includes a scraper or a wire brush and scrapes the coating layer off the base film.
[0038]
[11] The coating removal device according to [8], wherein:
[0039] The removal mechanism is a mechanism including a sandblasting device and scraping off the coating layer from the base film using a sandblasting material.
[0040]
[12] The coating removal device according to any one of [8] to
[11] , wherein:
[0041] It also has a steam blowing mechanism.
[0042] The water vapor blowing mechanism is a mechanism for blowing superheated water vapor toward the coating layer of the stretched laminated film.
[0043]
[13] The coating removal device according to any one of [8] to
[12] , wherein:
[0044] The stretching mechanism includes a heating mechanism for heating the laminated film.
[0045]
[14] The coating removal device according to any one of [8] to
[13] , wherein:
[0046] The laminated film is used for manufacturing a ceramic green sheet and is a laminated film after the ceramic green sheet is peeled off from the laminated film.
[0047] According to one aspect of the present invention, a coating layer removal method and a coating layer removal apparatus can be provided, which can easily remove the coating layer from a laminated film having a base film and a coating layer that is transported in a roll-to-roll manner. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1A This is an example of a cross-sectional view of a laminated film that can be used in the coating removal method of the first embodiment.
[0049] Figure 1B yes Figure 1A The laminated film shown is an example of a cross-sectional view of the laminated film after the laminated film is stretched in the longitudinal direction by the stretching step.
[0050] Figure 2 It is a microscope photograph showing a state where cracks are generated in the coating layer, and is a plan view of the laminated film observed from the coating layer side.
[0051] Figure 3 This is a schematic diagram showing an example of a coating removal device according to a second embodiment.
[0052] Figure 4 This is a schematic diagram showing an example of a coating removal device according to a third embodiment.
[0053] Figure 5 This is a schematic diagram showing an example of a coating removal device according to a fourth embodiment.
[0054] Figure 6 This is a schematic diagram showing an example of a coating removal device according to a fifth embodiment.
[0055] Figure 7 This is a schematic diagram showing an example of a coating removal device according to a sixth embodiment. DETAILED DESCRIPTION
[0056] [First embodiment]
[0057] (Coating removal method)
[0058] The coating removal method of the present embodiment comprises: a process of preparing a roll formed by winding a laminate film having a base film and a coating layer (hereinafter also referred to as a preparation process); a process of sending out the laminate film from the roll (hereinafter also referred to as a sending process); a process of stretching the laminate film after sending out (hereinafter also referred to as a stretching process); a process of removing the coating from the stretched laminate film (hereinafter also referred to as a removal process); and a process of rolling up the base film after the coating layer is removed into a roll (hereinafter also referred to as a winding process).
[0059] Figure 1A This is an example of a cross-sectional view of a laminated film 50 that can be used in the coating removal method of the first embodiment.
[0060] The laminated film 50 includes a base film 51 and a coating layer 52. In the laminated film 50, the base film 51 and the coating layer 52 are in direct contact with each other.
[0061] Figure 1B express Figure 1A The illustrated laminated film 50 is an example of a cross-sectional view of a laminated film 50A after the laminated film 50 is stretched in the longitudinal direction (transport direction) by a stretching step.
[0062] Figure 1B The figure shows a state where a plurality of cracks 522 are generated in the coating layer 52A of the stretched laminated film 50A.
[0063] In this embodiment, the stretching step is a step of causing cracks in the coating. Cause cracks in the coating to occur in the thickness direction of the coating, preferably until the cracks reach the interface with the substrate film (for example, Figure 1B The cracks generated in the coating are initially formed in a direction substantially perpendicular to the extension direction, and further cracks are generated in the extension direction by extension. Preferably, by extension, the coating on the substrate film is surrounded by cracks and becomes a small flake. Figure 2 It is a microscope photograph showing a state where cracks are generated in the coating layer, and is a plan view of the laminated film observed from the coating layer side.
[0064] In addition, there are cases where the impact caused by cracks in the coating layer causes partial peeling between the base film and the coating layer. Figure 2 In the microscope photograph of , the white part of the outer periphery of the polygon is the part where the coating peels off at the interface with the base film near the crack and air is drawn in. If such peeling occurs, the removal of the coating in the next step can be carried out more reliably, so it is preferred.
[0065] Furthermore, according to the coating removal method of the present embodiment, since each step is continuously performed in a roll-to-roll manner, the coating removal and the winding of the base film can be performed efficiently.
[0066] The coating removal method of the present embodiment can be implemented using, for example, the coating removal apparatus of any of the second to sixth embodiments.
[0067] First, a coating removal apparatus 100 according to a second embodiment will be described.
[0068] [Second embodiment]
[0069] [Coating removal device 100]
[0070] Figure 3 This is a schematic diagram of an example of a coating removal device 100 according to the second embodiment.
[0071] Hereinafter, the stretched laminated film is referred to as “stretched laminated film”, and the stretched coating layer is referred to as “stretched coating layer”.
[0072] Figure 3 to Figure 7 The X-axis, Y-axis, and Z-axis are respectively orthogonal to each other, the X-axis and the Y-axis are axes within a specified plane, and the Z-axis is an axis orthogonal to the specified plane.
[0073] The coating removal device 100 of the second embodiment is a coating removal device 100 for removing a coating 52 from a laminate film 50 having a substrate film 51 and a coating 52, and the coating removal device 100 comprises: a feeding mechanism 10 for feeding out the laminate film 50 from a roll 1 formed by winding the laminate film 50; a stretching mechanism 20 for stretching the laminate film 50 after feeding out; a removal mechanism 30 for removing the coating (the stretched coating 52A) from the stretched laminate film 50A; and a winding mechanism 40 for winding the substrate film 51 into a roll.
[0074] In the second embodiment, a case where the removal mechanism 30 includes the adhesive roll 5 will be described.
[0075] The laminated film 50 suitable for the removal device 100 is preferably a laminated film used in the manufacture of ceramic green sheets and after the ceramic green sheets are peeled off. The ceramic green sheets manufactured in this way are preferably used in the manufacture of multilayer ceramic capacitors (MLCC).
[0076] <Sending mechanism 10>
[0077] The feeding mechanism 10 includes a roll 1 formed by winding up the laminated film 50 , a support member (not shown) that rotatably supports the roll 1 , and a driving roller (not shown).
[0078] <Extension mechanism 20>
[0079] The stretching mechanism 20 includes: a first stretching roll 3A, a second stretching roll 3B arranged downstream of the first stretching roll 3A, a circumferential speed control mechanism 3C for controlling the circumferential speeds of the first stretching roll 3A and the second stretching roll 3B, and a first clamping roll 2A and a second clamping roll 2B respectively arranged opposite to the first stretching roll 3A and the second stretching roll 3B.
[0080] Drive motors M1 and M2 are connected to the shafts of the first and second reels 3A and 3B, respectively. The peripheral speed control mechanism 3C controls the peripheral speeds of the first and second reels 3A and 3B by controlling the drive motors M1 and M2. The peripheral speed control mechanism 3C is, for example, a computer.
[0081] The stretching mechanism 20 preferably includes a heating mechanism for heating the laminated film 50 .
[0082] The heating means is not particularly limited, and examples thereof include an infrared heater, a halogen heater, a UV lamp, and a hot air generating device.
[0083] From the viewpoint of easily stretching the base film, the heating mechanism is preferably arranged on the base film 51 side of the laminated film 50 to heat the laminated film 50 from the base film 51 side. The heating mechanism may also be arranged on the coating layer 52 side of the laminated film 50 to heat the laminated film 50 from the coating layer 52 side.
[0084] exist Figure 3 In this case, a heating mechanism 80 for heating the laminated film 50 from the base film 51 side is provided between the first stretching roll 3A and the second stretching roll 3B.
[0085] <Removal of mechanism 30>
[0086] The removal mechanism 30 is a mechanism that includes the adhesive roll 5 and transfers the coating layer (the coating layer 52A after extension) from the base film 51 to the adhesive roll 5 .
[0087] The adhesive roll 5 is, for example, a roll of an adhesive sheet 60 having a base sheet and an adhesive layer. The base sheet is not particularly limited, and examples thereof include paper and resin sheets. The adhesive layer is not particularly limited, and a known adhesive layer can be used.
[0088] The removal mechanism includes an adhesive roll 5 , an adhesive paper take-up roll 6 , and a guide roll 7 disposed opposite to the adhesive roll 5 .
[0089] exist Figure 3 In this case, the coating layer (the coating layer 52A after extension) is transferred to the adhesive layer of the adhesive sheet 60. The adhesive paper take-up roll 6 takes up the adhesive sheet to which the coating layer 52A is transferred (hereinafter also referred to as the coated adhesive sheet 61).
[0090] <Reeling mechanism 40>
[0091] The winding mechanism 40 includes a winding roll 4 for winding the base film 51 into a roll, a support member (not shown) for rotatably supporting the winding roll 4 , and a driving roller (not shown).
[0092] When the coating removal apparatus 100 of the second embodiment is used, the coating removal method of the first embodiment is implemented through the following steps, for example.
[0093] <Preparation process>
[0094] The preparation step is a step of preparing the roll 1 in which the laminated film 50 having the base film 51 and the coating layer 52 is wound.
[0095] The preparation step may be a step of merely preparing a roll (roll 1 wound up from the laminated film 50 ) manufactured in advance, or may be a step of manufacturing the roll 1 wound up from the laminated film 50 .
[0096] The laminated film 50 is preferably a laminated film used in the production of ceramic green sheets and obtained after the ceramic green sheets are peeled off.
[0097] <Sending process>
[0098] The feeding step is a step of feeding out the laminated film 50 from the roll 1 formed by winding the laminated film 50 .
[0099] exist Figure 3 In the case of the stacked film 50 fed from the roll 1 by the feeding mechanism 10 is directed toward the first clamping roll 2A ( Figure 3 The X-axis direction is used for transportation.
[0100] exist Figure 3 In the enlarged view of the laminated film in the region R1, for example, Figure 1A As shown, in the laminated film 50 delivered from the roll 1, the base film 51 and the coating layer 52 are Figure 3 The layers are stacked sequentially in region R1 toward the Z-axis direction.
[0101] <Stretching process>
[0102] The stretching step is a step of stretching the laminated film 50 .
[0103] exist Figure 3 In the case of the laminate film 50 fed from the roll 1, after passing through the first clamping roll 2A and the first stretching roll 3A in a substantially S-shaped manner, the laminate film 50 is stretched in the region R2 where it is fed from the first stretching roll 3A to the second stretching roll 3B. The stretching process generates cracks in the coating layer 52. Figure 3 In the enlarged view of the stretched laminated film 50A in the region R2, for example, Figure 1B In addition, the state of the stretched laminated film 50A in the region R2 as viewed from the Z axis is as follows. Figure 2 shown.
[0104] As a method of stretching the laminated film 50, for example, there can be mentioned:
[0105] A method of controlling the peripheral speed of the second stretching roll 3B disposed on the downstream side of the conveying path to be faster than the peripheral speed of the first stretching roll 3A disposed on the upstream side of the conveying path, and
[0106] A method in which one or more other stretching rolls are provided between the first stretching roll 3A and the second stretching roll 3B, and the laminated film 50 is transported so as to be wound around the first stretching roll 3A, the other stretching rolls, and the second stretching roll 3B.
[0107] As a method of stretching the laminated film 50, a method of controlling the peripheral speed of the second stretching roll 3B provided on the downstream side of the conveyance path to be faster than the peripheral speed of the first stretching roll 3A provided on the upstream side of the conveyance path is preferred.
[0108] The stretching step is preferably performed while the laminated film 50 is heated.
[0109] exist Figure 3In the case of , the laminated film 50 is heated from the base film 51 side using the heating mechanism 80 in the region R2 where the laminated film 50 is conveyed from the first stretching roll 3A to the second stretching roll 3B.
[0110] By performing the stretching step while heating the laminated film 50 , cracks are more likely to be generated in the coating layer 52 than when the stretching step is performed at room temperature.
[0111] For example, when a laminated film obtained by peeling off a ceramic green sheet is used as the laminated film 50 , the heating in the stretching step exhibits a greater effect.
[0112] The laminated film after peeling off the ceramic green sheets, that is, the stamping process is applied to each ceramic green sheet in the used laminated film, which may produce a tiny cut on the remaining surface, and the laminated film is easily broken starting from the tiny cut. Therefore, in the case of using the used laminated film, it is difficult to break the laminated film by performing the stretching process while heating the laminated film. As a result, the ceramic green sheets formed on the laminated film are cut to a specified size, and even in the case of using the laminated film after peeling off the ceramic green sheets, the removal of the coating and the winding of the base film can be completed without any problem by the roll-to-roll method.
[0113] The heating temperature and heating time when the laminated film 50 is heated are determined by the materials of the base film 51 and the coating layer 52 .
[0114] The heating of the laminated film 50 is preferably performed at a temperature equal to or higher than the glass transition temperature Tg1 of the base film 51 for the following reason.
[0115] The glass transition temperature Tg1 of the base film 51 and the glass transition temperature Tg2 of the coating layer 52 in the laminated film 50 are obtained by the method specified in JIS K7121 (2012) and measured using a differential scanning calorimeter (DSC). In order to easily extend the base film 51 without breaking and easily break the coating layer 52, the temperature during extension is preferably not less than the glass transition temperature Tg1 of the base film 51, and more preferably not less than the glass transition temperature Tg1 of the base film 51 and not more than the glass transition temperature Tg2 of the coating layer 52.
[0116] <Removal process>
[0117] The removal step is a step of removing the coating layer (coating layer 52A after extension) from the extended laminated film 50A.
[0118] exist Figure 3 In the case of , the removal step is a step of transferring the stretched coating layer 52A from the base film 51 to the adhesive roll 5 .
[0119] The laminated film 50A stretched by the stretching process passes through the second stretching roll 3B and the second clamping roll 2B in a substantially S-shaped manner, and is then conveyed toward the adhesive roll 5. When the stretched laminated film 50A passes between the adhesive roll 5 and the guide roll 7, the coating layer 52A is transferred from the base film 51 to the adhesive layer of the adhesive sheet 60. The adhesive sheet (coating tape adhesive sheet 61) to which the coating layer 52A is transferred is taken up by the adhesive paper take-up roll 6.
[0120] <Coiling process>
[0121] The winding step is a step of winding the base film 51 after the coating layer (the stretched coating layer 52A) is removed into a roll.
[0122] exist Figure 3 In the case of , the base film 51 is wound up by the winding roll 4 into a roll shape.
[0123] [Third embodiment]
[0124] [Coating removal device 100A]
[0125] A coating removal apparatus 100A according to a third embodiment will be described.
[0126] In the third embodiment, the differences from the second embodiment will be mainly described, and the description of the same matters will be omitted or simplified by attaching the same reference numerals or the like.
[0127] Figure 4 This is a schematic diagram of an example of a coating removal apparatus 100A according to a third embodiment. Figure 4 The removal device 100A shown is the same as the second embodiment except that the removal mechanism is different from the removal device 100 described in the second embodiment.
[0128] <Removal mechanism 30A>
[0129] The removal mechanism 30A is a mechanism that includes a scraper 5A and scrapes off the extended coating layer 52A from the base film 51 .
[0130] The scraper 5A is provided at an arbitrary position on the downstream side of the laminated film 50A stretched in the stretching step.
[0131] exist Figure 4 In the case of , the scraper 5A is provided to contact the laminated film (laminated film 50A after stretching) on the downstream side of the guide roll 7. The removal mechanism 30A includes the scraper 5A for scraping off the stretched coating 52A and a receiving pan 63 for collecting the scraped coating 52A.
[0132] The material of the scraper 5A is not particularly limited.
[0133] When the coating removal apparatus 100A of the third embodiment is used, the coating removal method of the first embodiment is implemented through the following steps, for example.
[0134] The following description will focus on points different from the second embodiment.
[0135] <Removal process>
[0136] The removal step is a step of scraping off the stretched coating layer 52A from the base film 51 using the scraper 5A.
[0137] The coating scraped off by the scraper 5A (the coating 52A after extension) is collected in the receiving pan 63 .
[0138] [Fourth embodiment]
[0139] [Coating removal device 100B]
[0140] A coating removal apparatus 100B according to a fourth embodiment will be described.
[0141] In the fourth embodiment, the description will be mainly focused on the differences from the second embodiment, and the description of the same matters will be omitted or simplified by assigning the same reference numerals to the same matters.
[0142] Figure 5 This is a schematic diagram of an example of a coating removal apparatus 100B according to a fourth embodiment. Figure 5 The removal device 100B shown is the same as the second embodiment except that the removal mechanism is different from the removal device 100 described in the second embodiment.
[0143] <Removal mechanism 30B>
[0144] The removal mechanism 30B is a mechanism that includes a wire brush 5B and scrapes off the extended coating layer 52A from the base film 51 .
[0145] The wire brush 5B is rotatably provided at an arbitrary position on the downstream side of the stretched laminated film 50A.
[0146] exist Figure 5 In the case of, the wire brush 5B is disposed opposite to the guide roll 7. The removal mechanism 30B includes the wire brush 5B for scraping off the stretched coating 52A, and a receiving pan 63 for recovering the scraped coating 52A.
[0147] The material of the wire brush 5B is not particularly limited.
[0148] like Figure 5As shown, by arranging the wire brush 5B and the guide roll 7 to face each other in the horizontal direction and scraping the coating 52A downward, the coating 52A can be effectively recovered.
[0149] When the coating removal apparatus 100B of the fourth embodiment is used, the coating removal method of the first embodiment is implemented through the following steps, for example.
[0150] The following description will focus on points different from the second embodiment.
[0151] <Removal process>
[0152] The removal step is a step of scraping off the stretched coating layer 52A from the base film 51 using the wire brush 5B.
[0153] When the stretched laminate film 50A passes between the wire brush 5B and the guide roll 7, the coating (stretched coating 52A) is scraped off from the base film 51 by the rotation of the wire brush 5B. The scraped coating (stretched coating 52A) is collected on the receiving pan 63.
[0154] [Fifth embodiment]
[0155] [Coating removal device 100C]
[0156] A coating removal apparatus 100C according to a fifth embodiment will be described.
[0157] In the fifth embodiment, the description will be mainly focused on the points different from the second embodiment, and the description of the same matters will be omitted or simplified by assigning the same reference numerals to the same matters.
[0158] Figure 6 This is a schematic diagram of an example of a coating removal apparatus 100C according to a fifth embodiment. Figure 6 The removal device 100C shown is the same as the second embodiment except that the removal mechanism is different from the removal device 100 described in the second embodiment.
[0159] <Removal mechanism 30C>
[0160] The removal mechanism 30C is a mechanism that includes a sandblasting device 5C and scrapes away the stretched coating layer 52A from the base film 51 using a sandblasting material.
[0161] The sandblasting device 5C is provided at an arbitrary position on the downstream side of the stretched laminated film 50A, and scrapes off the coating layer 52A by blowing sandblasting material toward the coating layer (the stretched coating layer 52A).
[0162] exist Figure 5In the case of , the removal mechanism 30C includes a sandblasting device 5C and a receiving pan 63 for recovering the removed coating 52A together with the sandblasting material (not shown).
[0163] As the sand blasting device 5C, a well-known sand blasting device can be used.
[0164] Examples of the blasting material include silicon dioxide particles, calcium carbonate particles, silicon carbide particles, aluminum oxide particles, dry ice particles, and melamine resin particles. When dry ice particles are used as the blasting material, since the dry ice particles disappear after the blasting process, it is not necessary to remove the particles, which is preferred. The particle size of the blasting material is preferably 5 μm or more and 40 μm or less.
[0165] The blowing conditions of the blasting material are determined by the material of the coating.
[0166] When the coating removal apparatus 100C of the fifth embodiment is used, the coating removal method of the first embodiment is implemented through the following steps, for example.
[0167] The following description will focus on points different from the second embodiment.
[0168] <Removal process>
[0169] The removal step is a step of scraping off the coating layer (coating layer 52A after extension) from the base film 51 by a sandblasting material.
[0170] When the stretched laminated film 50A passes between the sandblasting device 5C and the guide roll 7, the stretched coating layer 52A is scraped off from the base film 51 by blowing sandblasting material (not shown) from the sandblasting device 5C. The scraped coating layer (stretched coating layer 52A) is recovered on the receiving pan 63 together with the sandblasting material.
[0171] [Sixth embodiment]
[0172] [Coating removal device 100D]
[0173] A coating removal apparatus 100D according to a sixth embodiment will be described.
[0174] In the sixth embodiment, the description will be mainly focused on the differences from the second embodiment, and the description of the same matters will be omitted or simplified by assigning the same reference numerals to the same matters.
[0175] Figure 7 This is a schematic diagram of an example of a coating removal apparatus 100D according to the sixth embodiment.
[0176] Figure 7The removal device 100D shown is the same as the second embodiment except that a water vapor blowing mechanism is provided between the stretching mechanism and the removal mechanism, with respect to the removal device 100 described in the second embodiment.
[0177] <Steam blowing mechanism>
[0178] The water vapor blowing mechanism is a mechanism for blowing superheated water vapor toward the coating layer of the stretched laminate film 50A (the stretched coating layer 52A).
[0179] The water vapor blowing mechanism may include a heater for heating the water vapor and a water vapor blowing nozzle for blowing out the superheated water vapor.
[0180] The water vapor blowing mechanism is provided between the extending mechanism 20 and the removing mechanism 30 .
[0181] exist Figure 7 In the case of, the water vapor blowing mechanism is a superheater 70 having a plurality of water vapor blowing nozzles 70a and a treatment chamber 72. The superheater 70 is disposed between the boiler 71 and the treatment chamber 72. The superheater 70 is connected to the boiler 71, heats the water vapor generated in the boiler 71 to generate superheated water vapor, and blows the superheated water vapor from the water vapor blowing nozzles 70a toward the coating (the coating 52A after extension) in the treatment chamber 72.
[0182] When the coating removal apparatus 100D of the sixth embodiment is used, the coating removal method of the first embodiment is implemented through the following steps, for example.
[0183] The following description will focus on points different from the second embodiment.
[0184] <Steam Blowing Process>
[0185] The steam blowing step is a step of blowing superheated steam toward the coating layer of the stretched laminate film 50A (the stretched coating layer 52A) after the stretching step and before the removal step.
[0186] exist Figure 7 In the case of the stretched laminated film 50A, after the superheated water vapor is blown toward the coating layer 52A from the water vapor blowing nozzle 70a, the laminated film 50A is discharged from the processing chamber 72 and rapidly cooled. Due to the rapid cooling, the coating layer 52A is easily deformed due to the difference in thermal expansion coefficient between the coating layer 52A and the base film 51, and the interface peeling of the coating layer 52A is promoted. As a result, in the subsequent removal process, the coating layer 52A is easily removed from the base film 51.
[0187] The temperature of the superheated water vapor is preferably 100°C to 450°C, more preferably 150°C to 400°C, and further preferably 200°C to 350°C.
[0188] The blowing time of the superheated water vapor is determined by the material of the coating layer and the conveying speed of the laminated film 50 .
[0189] [Variations of Embodiments]
[0190] In the removal devices of the second embodiment to the sixth embodiment, the heating mechanism 80 is provided between the delivery mechanism 10 and the first stretching roll 3A. That is, the heating mechanism 80 is preferably configured to heat the laminated film 50 before the laminated film 50 is stretched. In this case, the removal method of the first embodiment further includes a step of heating the laminated film 50 after the delivery step and before the stretching step. By heating the laminated film 50 before the stretching step, cracks are easily generated in the coating layer 52.
[0191] The present invention is not limited to the above-described embodiments, and the present invention may include modifications and improvements within the scope of achieving the purpose of the present invention.
[0192] The structure of the laminated film used for the coating removal method of the first embodiment and the coating removal apparatuses of the second to sixth embodiments will be described.
[0193] 〔Laminated film〕
[0194] The laminated film used in any of the above-mentioned embodiments includes a base film and a coating layer.
[0195] The coating layer may be a single layer or a multilayer composed of two or more coating layers of the same or different types. In addition, the coating layer may be formed on both sides of the base film.
[0196] From the viewpoint of easily removing the coating from the laminated film and recycling the remaining substrate film, in the laminated film, the substrate film and the coating are preferably directly laminated. Here, "directly laminated" means: for example, there is no other layer between the substrate film and the coating, and the substrate film and the coating are in direct contact with each other.
[0197] <Base film>
[0198] As the base film, a resin film produced from a resin component to be recovered is used.
[0199] As the resin film, polyester films such as polyethylene terephthalate film, polybutylene terephthalate, and polyethylene naphthalate; polyolefin films such as polyethylene film and polypropylene film; polyimide film; polyamide film; polycarbonate film; polyacetate film; ethylene-vinyl acetate copolymer (EVA) film; ethylene-(meth)acrylic acid copolymer film; ethylene-(meth)acrylate copolymer film; cycloolefin polymer film; polyurethane film; polyphenylene sulfide film; cellophane; and the like can be used.
[0200] Among these, polyester films are preferred from the viewpoint of heat resistance and strength. As polyester films, polyester films mainly composed of any one of polyethylene terephthalate, polybutylene terephthalate and polyethylene naphthalate are preferred from the viewpoint of resin recovery and easy regeneration.
[0201] In addition, the resin film may contain known fillers, colorants, antistatic agents, antioxidants, organic lubricants, catalysts, etc. In addition, the resin film may be a transparent material, or may be colored as desired. In addition, surface treatments such as sputtering, corona discharge, flame, ultraviolet irradiation, electron beam irradiation, and etching such as oxidation may be applied in advance to at least one surface of the substrate film as needed.
[0202] The thickness of the substrate film is not particularly limited, but is preferably 10 μm to 500 μm, more preferably 15 μm to 300 μm, and further preferably 20 μm to 200 μm from the viewpoint of strength and rigidity.
[0203] <Coating>
[0204] The coating layer is preferably a functional layer. As the functional layer, for example, a release agent layer, a printing layer, a hard coating layer, an easy adhesion layer and an adhesive layer can be cited. Among these, the coating layer is preferably a release agent layer.
[0205] When the coating layer is a release agent layer, the release agent layer is preferably a layer formed of a release agent composition.
[0206] The release agent composition used for forming the release agent layer is not particularly limited as long as it has release properties, and for example, a release agent composition containing silicone compounds; fluorine compounds; compounds containing long-chain alkyl groups; thermoplastic resin materials such as olefin resins and diene resins as main components can be used. In addition, a release agent composition containing energy-ray curable or thermosetting resins as main components is preferably used. These release agent compositions can be used alone or in combination of two or more.
[0207] In the release agent composition having an organosilicon compound as a main component, the organosilicon compound may include an organosilicon compound having an organopolysiloxane as a basic skeleton. In addition, the organosilicon compound may include heat-curing organosilicon compounds such as addition reaction type and condensation reaction type, and energy ray-curing organosilicon compounds such as ultraviolet curing type and electron beam curing type.
[0208] In the release agent composition containing a fluorine compound as a main component, examples of the fluorine compound include fluorosilicone compounds, fluoroboron compounds, and poly(perfluoroalkylene ether) chain-containing compounds.
[0209] In the stripping agent composition containing a long-chain alkyl group-containing compound as a main component, examples of the long-chain alkyl group-containing compound include: polyvinyl carbamate obtained by reacting a polyvinyl alcohol polymer with a long-chain alkyl isocyanate, an alkyl urea derivative obtained by reacting polyethylene imine with a long-chain alkyl isocyanate, or a copolymer of a long-chain alkyl (meth)acrylate, etc. Furthermore, among the alkyd resins obtained by the condensation reaction of a polyol and a polyacid, a long-chain alkyl-modified alkyd resin using a long-chain fatty acid as a modifier can be used.
[0210] As a stripper composition with energy-ray curing resin as the main component, for example, it is preferred to include an energy-ray curing compound and polyorganosiloxane having a reactive functional group selected from (meth) acryloyl, alkenyl and maleimide. In the stripper layer formed by the stripper composition, since energy-ray curing compounds and polyorganosiloxane with different molecular structures, polarities and molecular weights are used, the components from the polyorganosiloxane are segregated near the outer surface of the stripper layer before curing, and then the segregation is fixed by energy-ray curing. Thus, the stripping property of the stripper layer can be improved. As a stripper composition with energy-ray curing resin as the main component, a photopolymerization initiator can be further contained.
[0211] As a stripper composition with a thermosetting resin as the main component, for example, a stripper composition with a melamine resin as the main component and a stripper composition with an epoxy resin as the main component can be cited. As a stripper composition with a melamine resin as the main component, a composition comprising a melamine resin as a main agent, an acid catalyst for thermosetting the melamine resin, and a polyorganosiloxane that imparts stripping properties to the stripper layer can be cited. In addition, as a stripper composition with an epoxy resin as the main component, a composition comprising an epoxy resin as a main agent, an acid or alkaline thermosetting catalyst for thermosetting the epoxy resin, and a polyorganosiloxane that imparts stripping properties to the stripper layer can be cited. Before curing, the components from the polyorganosiloxane are segregated near the outer surface of the stripper layer, and then cured, and the segregation is fixed. Thus, the stripping properties of the stripper layer can be improved.
[0212] In addition, the coating layer may contain other additives in addition to the resin component, such as anti-aging agents, light stabilizers, flame retardants, conductive agents, antistatic agents, and plasticizers.
[0213] The thickness of the coating layer can be appropriately selected and is not particularly limited, but is, for example, preferably 0.02 μm to 5 μm, more preferably 0.03 μm to 2 μm, and further preferably 0.05 μm to 1.5 μm.
[0214] The laminated film used in each embodiment is usually used for the purpose of protecting the surface of other functional sheets or various components for specific purposes, such as during the manufacture, transportation and storage of these functional sheets or components. In fact, after playing the role of protecting these components, most of them are peeled off from the surface and discarded. Therefore, by using the laminated film, the coating and the substrate film can be easily separated from the laminated film, so from the perspective of resource protection and environmental protection, this is a highly contributing use.
[0215] Description of Reference Numerals
[0216] 1…roll, 2A…first clamping roll, 2B…second clamping roll, 3A…first stretching roll, 3B…second stretching roll, 3C…circumferential speed control mechanism, 4…winding roll, 5…adhesive roll, 5A…scraper, 5B…wire brush, 5C…sandblasting device, 6…adhesive paper winding roll, 7…guide roll, 10…feeding mechanism, 20…stretching mechanism, 30, 30A, 30B, 30C…removal mechanism, 40…winding mechanism, 50, 50A…laminated film, 51…base film, 52, 52A…coating, 60…adhesive sheet, 61…coating with adhesive sheet, 63…receiving tray, 70…superheater, 70a…steam blowing nozzle, 71…boiler, 72…processing chamber, 80…heating mechanism, 100, 100A, 100B, 100C, 100D…removal device, 522…crack.
Claims
1. A method for removing a coating, wherein: have: A step of preparing a roll formed by winding a laminated film having a base film and a coating layer; a step of feeding the laminated film from the roll; A step of stretching the laminated film after it is sent out; A step of removing the coating layer from the stretched laminated film; A step of winding the base film after the coating layer is removed into a roll.
2. The method for removing a coating according to claim 1, wherein: The step of removing the coating layer is a step of transferring the coating layer from the base film to the adhesive roll.
3. The method for removing a coating according to claim 1, wherein: The step of removing the coating layer is a step of scraping the coating layer off the base film using a scraper or a wire brush.
4. The method for removing a coating according to claim 1, wherein: The step of removing the coating layer is a step of scraping the coating layer off the base film using a sandblasting material.
5. The method for removing a coating according to any one of claims 1 to 4, wherein: The step of stretching the laminated film is performed while heating the laminated film.
6. The method for removing a coating according to any one of claims 1 to 4, wherein: After the step of stretching the laminated film and before the step of removing the coating layer, there is a step of blowing superheated water vapor toward the coating layer of the stretched laminated film.
7. The method for removing a coating according to any one of claims 1 to 4, wherein: The laminated film is used for manufacturing a ceramic green sheet and is the laminated film after the ceramic green sheet is peeled off.
8. A coating removal device for removing the coating from a laminated film having a substrate film and a coating, wherein: The coating removal device comprises: a feeding mechanism for feeding the laminated film from a roll formed by winding the laminated film; A stretching mechanism, which stretches the laminated film after being sent out; a removing mechanism for removing the coating from the stretched laminated film; A winding mechanism winds up the base film into a roll.
9. The coating removal device according to claim 8, wherein: The removal mechanism is a mechanism including an adhesive roll and transferring the coating layer from the base film to the adhesive roll.
10. The coating removal device according to claim 8, wherein: The removal mechanism is a mechanism that includes a scraper or a wire brush and scrapes the coating layer off the base film.
11. The coating removal device according to claim 8, wherein: The removal mechanism is a mechanism including a sandblasting device and scraping off the coating layer from the base film using a sandblasting material.
12. The coating removal device according to any one of claims 8 to 11, wherein: It also has a steam blowing mechanism. The water vapor blowing mechanism is a mechanism for blowing superheated water vapor toward the coating layer of the stretched laminated film.
13. The coating removal device according to any one of claims 8 to 11, wherein: The stretching mechanism includes a heating mechanism for heating the laminated film.
14. The coating removal device according to any one of claims 8 to 11, wherein: The laminated film is used for manufacturing a ceramic green sheet and is a laminated film after the ceramic green sheet is peeled off from the laminated film.