Thermoplastic polyurethane resin, film, and coating protective film

By adjusting the ratio of polyisocyanate components and polyols, an appropriate polyurethane structure is formed, which solves the problem of poor fingerprint recovery of thermoplastic polyurethane resin film, and achieves a good balance between the stretching characteristics, heat resistance and fingerprint recovery of the film. .

CN118974132APending Publication Date: 2024-11-15MITSUI CHEMICALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380032076.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-27
Filing Date
2023-05-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing thermoplastic polyurethane resin films have poor performance in fingerprint recovery, and it is difficult to take into account both the telescopic properties, heat resistance and fingerprint recovery.

Method used

By adjusting the ratio of 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane in the polyisocyanate component and using crystalline and low molecular weight polyols, a crystalline and low molecular weight polyol is formed Appropriate polyurethane structure to improve fingerprint recovery and heat resistance of the film.

Benefits of technology

A good balance between the expansion characteristics, heat resistance and fingerprint recovery of the thermoplastic polyurethane resin film is achieved, and the overall performance of the film is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005067876210000241
    Figure BDA0005067876210000241
  • Figure BDA0005067876210000251
    Figure BDA0005067876210000251
  • Figure BDA0005067876210000261
    Figure BDA0005067876210000261
Patent Text Reader

Abstract

The thermoplastic polyurethane resin includes a reaction product of a polyisocyanate component and a polyol component. The polyisocyanate component contains 1, 4-bis (isocyanatomethyl) cyclohexane and 1, 3-bis (isocyanatomethyl) cyclohexane, and is characterized in that: the polyisocyanate component contains 1, 4-bis (isocyanatomethyl) cyclohexane and 1, 3-bis (isocyanatomethyl) cyclohexane; the polyol component includes a polycarbonate polyol and a low molecular weight polyol. The polycarbonate polyol contains a crystalline polycarbonate polyol that is solid at 25 DEG C. The amount of 1, 4-bis (isocyanatomethyl) cyclohexane is 50 to 90 mol% and the amount of 1, 3-bis (isocyanatomethyl) cyclohexane is 10 to 50 mol% with respect to the total amount of 1, 4-bis (isocyanatomethyl) cyclohexane and 1, 3-bis (isocyanatomethyl) cyclohexane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermoplastic polyurethane resin, a film and a coating protective film. Background Art

[0002] Thermoplastic polyurethane resin (TPU) can be obtained by the reaction of polyisocyanate, macromolecular polyol and low molecular weight polyol. Thermoplastic polyurethane resin is formed into a film, for example. The film-like thermoplastic polyurethane resin is used as a base film in a paint protection film (Paint Protection Film (PPF), laminated film) for protecting the painted surface of an automobile.

[0003] As a base film of a paint protection film (PPF), for example, the following film is known. The film contains a thermoplastic polyurethane resin. The thermoplastic polyurethane resin contains a reaction product of a polyisocyanate component and a polyol component. The polyisocyanate component contains 1,4-bis(isocyanatemethyl)cyclohexane. The polyol component contains an amorphous polycarbonate diol that is liquid at 25°C and a low molecular weight diol having 2 to 6 carbon atoms (for example, see Patent Document 1).

[0004] Such a film has excellent stretching characteristics (restoration force) and heat resistance.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2019 / 069802 Summary of the invention

[0008] Problems to be solved by the invention

[0009] On the other hand, the film is also required to have recovery properties against adhesion of fingerprints (fingerprint recovery properties). In this regard, the fingerprint recovery properties of the above-mentioned films are sometimes insufficient.

[0010] The present invention provides a thermoplastic polyurethane resin having a combination of stretching characteristics (restoring force), heat resistance and fingerprint restoring properties, and a film and a paint protection film comprising the thermoplastic polyurethane resin.

[0011] Means for solving problems

[0012] The present invention [1] includes a thermoplastic polyurethane resin comprising a reaction product of a polyisocyanate component and a polyol component, wherein the polyisocyanate component comprises 1,4-bis(isocyanatemethyl)cyclohexane and 1,3-bis(isocyanatemethyl)cyclohexane, the polyol component comprises a polycarbonate polyol and a low molecular weight polyol, the polycarbonate polyol comprises a crystalline polycarbonate polyol that is solid at 25° C., and the ratio of 1,4-bis(isocyanatemethyl)cyclohexane is 50 mol % to 90 mol % and the ratio of 1,3-bis(isocyanatemethyl)cyclohexane is 10 mol % to 50 mol % based on the total amount of 1,4-bis(isocyanatemethyl)cyclohexane and 1,3-bis(isocyanatemethyl)cyclohexane.

[0013] The present invention [2] comprises the thermoplastic polyurethane resin described in the above [1], wherein the polycarbonate polyol is composed of the crystalline polycarbonate polyol.

[0014] The present invention [3] comprises the thermoplastic polyurethane resin according to [1] or [2] above, wherein the thermoplastic polyurethane resin has a hard segment concentration of 18% by mass or more and 35% by mass or less.

[0015] The present invention [4] comprises the thermoplastic polyurethane resin according to any one of [1] to [3] above, wherein the polycarbonate polyol comprises a first polycarbonate polyol having a number average molecular weight of 1200 or less and a second polycarbonate polyol having a number average molecular weight of 1800 or more.

[0016] The present invention [5] includes a film comprising the thermoplastic polyurethane resin according to any one of the above [1] to [4].

[0017] The present invention [6] includes a paint protection film comprising a release layer, an adhesive layer disposed on at least one surface of the release layer, and a base film layer disposed on at least one surface of the adhesive layer, wherein the base film layer comprises the film described in [5] above.

[0018] Effects of the Invention

[0019] The raw material components of the thermoplastic polyurethane resin of the present invention contain 1,4-bis(isocyanatemethyl)cyclohexane, a crystalline polycarbonate polyol, and a polyol component containing a low molecular weight polyol at predetermined ratios.

[0020] 1,4-bis(isocyanatomethyl)cyclohexane has relatively high crystallinity. In addition, the low molecular weight polyol forms a hard segment, thereby improving crystallinity. In addition, the crystalline polycarbonate polyol has relatively high crystallinity.

[0021] In addition, the raw material component contains 1,3-bis(isocyanatemethyl)cyclohexane. 1,3-bis(isocyanatemethyl)cyclohexane has relatively low crystallinity.

[0022] In addition, among the raw material components, the ratio of 1,4-bis(isocyanatemethyl)cyclohexane to 1,3-bis(isocyanatemethyl)cyclohexane is adjusted to be within a predetermined range.

[0023] That is, the crystallinity of the polyurethane structure is adjusted by the raw material components. As a result, the thermoplastic polyurethane resin has a good balance of stretching characteristics (restoring force), heat resistance and fingerprint recovery.

[0024] Furthermore, since the film and the paint protection film of the present invention contain the above-mentioned thermoplastic polyurethane resin, they have both fingerprint recovery properties, stretch characteristics (restoration force), and heat resistance in a well-balanced manner. DETAILED DESCRIPTION

[0025] The thermoplastic polyurethane resin of the present invention can be obtained by reacting a polyisocyanate component with a polyol component. In other words, the thermoplastic polyurethane resin is a reaction product of a polyisocyanate component and a polyol component.

[0026] 1. Polyisocyanate component

[0027] (1) Bis(isocyanatemethyl)cyclohexane

[0028] The polyisocyanate component contains bis(isocyanatemethyl)cyclohexane (H6XDI) as an essential component. The bis(isocyanatemethyl)cyclohexane contains 1,4-bis(isocyanatemethyl)cyclohexane and 1,3-bis(isocyanatemethyl)cyclohexane.

[0029] 1,4-bis(isocyanate methyl)cyclohexane (1,4-H6XDI) has stereoisomers. Examples of the stereoisomers include cis-1,4-bis(isocyanate methyl)cyclohexane (hereinafter referred to as cis 1,4 isomer) and trans-1,4-bis(isocyanate methyl)cyclohexane (hereinafter referred to as trans 1,4 isomer).

[0030] 1,4-bis(isocyanatemethyl)cyclohexane contains, for example, a trans-1,4-isomer (trans-isomer) and a cis-1,4-isomer (cis-isomer). The total amount of the trans-1,4-isomer and the cis-1,4-isomer is 100 mol%.

[0031] The content ratio of the trans-1,4-isomer (trans-isomer) relative to the total mole of 1,4-bis(isocyanatemethyl)cyclohexane is, for example, 60 mol% or more, preferably 70 mol% or more, more preferably 75 mol% or more, and further preferably 80 mol% or more. In addition, the content ratio of the trans-1,4-isomer (trans-isomer) relative to the total mole of 1,4-bis(isocyanatemethyl)cyclohexane is, for example, 99.5 mol% or less, preferably 99 mol% or less, more preferably 96 mol% or less, and further preferably 90 mol% or less.

[0032] In other words, the content ratio of the cis-1,4-isomer (cis-isomer) relative to the total mole of 1,4-bis(isocyanatemethyl)cyclohexane is, for example, 0.5 mol% or more, preferably 1 mol% or more, more preferably 4 mol% or more, and further preferably 10 mol% or more. In addition, the content ratio of the cis-1,4-isomer (cis-isomer) relative to the total mole of 1,4-bis(isocyanatemethyl)cyclohexane is, for example, 40 mol% or less, preferably 30 mol% or less, more preferably 25 mol% or less, and further preferably 20 mol% or less.

[0033] 1,4-bis(isocyanate methyl)cyclohexane can be produced by a known method. The production method of 1,4-bis(isocyanate methyl)cyclohexane is described in, for example, International Publication No. 2009 / 051114 and International Publication No. 2019 / 069802.

[0034] 1,4-bis(isocyanate methyl)cyclohexane can be a monomer or a modified product. As a modified product, for example, uretdione modified products, isocyanurate modified products, imino oxadiazinedione, biuret modified products, allophanate modified products, polyol adducts, oxadiazinetrione modified products, and carbodiimide modified products can be cited. They can be used alone or in combination of two or more. 1,4-bis(isocyanate methyl)cyclohexane is preferably a monomer.

[0035] There are no particular limitations on 1,3-bis(isocyanatemethyl)cyclohexane (1,3-H6XDI), and known 1,3-bis(isocyanatemethyl)cyclohexane can be used.

[0036] 1,3-bis(isocyanate methyl)cyclohexane can be a monomer or a modified product. As a modified product, for example, uretdione modified products, isocyanurate modified products, imino oxadiazinedione, biuret modified products, allophanate modified products, polyol adducts, oxadiazinedione modified products, and carbodiimide modified products can be cited. They can be used alone or in combination of two or more. 1,3-bis(isocyanate methyl)cyclohexane is preferably a monomer.

[0037] In order to improve the expansion and contraction characteristics (restoration force), heat resistance and fingerprint recovery of the thermoplastic polyurethane resin in a well-balanced manner, 1,4-bis(isocyanatemethyl)cyclohexane and 1,3-bis(isocyanatemethyl)cyclohexane are used in combination at a predetermined ratio.

[0038] More specifically, the ratio of 1,4-bis(isocyanate methyl)cyclohexane to the total amount of 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane is 50 mol% or more, preferably 55 mol% or more, more preferably 60 mol% or more, and further preferably 65 mol% or more. In addition, the ratio of 1,4-bis(isocyanate methyl)cyclohexane to the total amount of 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane is 90 mol% or less, preferably 85 mol% or less, more preferably 80 mol% or less, and further preferably 75 mol% or less.

[0039] In addition, the ratio of 1,3-bis(isocyanate methyl)cyclohexane to the total amount of 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane is 10 mol% or more, preferably 15 mol% or more, more preferably 20 mol% or more, and further preferably 25 mol% or more. In addition, the ratio of 1,3-bis(isocyanate methyl)cyclohexane to the total amount of 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane is 50 mol% or less, preferably 45 mol% or less, more preferably 40 mol% or less, and further preferably 35 mol% or less.

[0040] (2) Other polyisocyanates

[0041] The polyisocyanate component may contain other polyisocyanates as optional components. Other polyisocyanates are polyisocyanates other than bis(isocyanatomethyl)cyclohexane.

[0042] Examples of other polyisocyanates include aliphatic polyisocyanates, alicyclic polyisocyanates (except bis(isocyanatemethyl)cyclohexane), aromatic polyisocyanates, and aromatic aliphatic polyisocyanates.

[0043] Examples of aliphatic polyisocyanates include pentamethylene diisocyanate (PDI) and hexamethylene diisocyanate (HDI). Examples of alicyclic polyisocyanates include isophorone diisocyanate (IPDI), norbornene diisocyanate (NBDI), and methylene bis(cyclohexyl isocyanate) (HDI). 12MDI). As aromatic polyisocyanates, for example, toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), toluidine diisocyanate (TODI), and naphthalene diisocyanate (NDI) can be mentioned. As aromatic aliphatic polyisocyanates, for example, xylylene diisocyanate (XDI) and tetramethylxylylene diisocyanate (TMXDI) can be mentioned. In addition, other polyisocyanates may be monomers or the above-mentioned modified products. They may be used alone or in combination of two or more.

[0044] The content ratio of other polyisocyanates relative to the total amount of the polyisocyanate component is, for example, 50 mass % or less, preferably 30 mass % or less, more preferably 10 mass % or less, particularly preferably 0 mass %.

[0045] That is, the content ratio of bis(isocyanate methyl)cyclohexane relative to the total amount of the polyisocyanate component is, for example, 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass. In other words, the polyisocyanate component is preferably composed of bis(isocyanate methyl)cyclohexane, and more preferably composed of 1,3-bis(isocyanate methyl)cyclohexane and 1,4-bis(isocyanate methyl)cyclohexane.

[0046] 2. Polyol ingredients

[0047] The polyol component contains a macromolecular polyol and a low molecular weight polyol. The polyol component is preferably composed of a macromolecular polyol and a low molecular weight polyol.

[0048] (1) Macromolecular polyols

[0049] Macromolecular polyols are organic compounds having two or more hydroxyl groups in the molecule and having a relatively high molecular weight. The term "relatively high molecular weight" means that the number average molecular weight is greater than 400.

[0050] The macropolyol contains a polycarbonate polyol as an essential component. The polycarbonate polyol contains a crystalline polycarbonate polyol as an essential component.

[0051] The crystalline polycarbonate polyol is a polycarbonate polyol that is solid at 25° C. The term “solid” means a state in which the viscosity at 25° C. measured by an E-type viscometer is greater than 500,000 mPa·s.

[0052] As crystalline polycarbonate polyols, for example, ring-opening polymers of ethylene carbonate using polyols as initiators can be cited. As for polyols as initiators, for example, dihydric alcohols having 2 to 8 carbon atoms and trihydric alcohols having 2 to 8 carbon atoms can be cited. As dihydric alcohols having 2 to 8 carbon atoms, for example, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, diethylene glycol, and triethylene glycol can be cited. As trihydric alcohols having 2 to 8 carbon atoms, for example, glycerol, trimethylolethane, and trimethylolpropane can be cited. They can be used alone or in combination of two or more. As polyols, dihydric alcohols can be preferably cited.

[0053] The method for ring-opening polymerization of ethylene carbonate using a polyol is not particularly limited, and a known method can be employed.

[0054] The number average molecular weight (molecular weight in terms of polystyrene) of the crystalline polycarbonate polyol is greater than 400, preferably greater than 500, and more preferably greater than 1000. In addition, the number average molecular weight (molecular weight in terms of polystyrene) of the crystalline polycarbonate polyol is, for example, 10,000 or less, preferably 8,000 or less, more preferably 5,000 or less, further preferably 3,000 or less, and particularly preferably 2,000 or less.

[0055] The average hydroxyl number of the crystalline polycarbonate polyol is, for example, 1.8 or more, and preferably 2 or more. In addition, the average hydroxyl number of the crystalline polycarbonate polyol is, for example, 4 or less, preferably 3 or less, and more preferably 2 or less. The average hydroxyl number of the crystalline polycarbonate polyol is particularly preferably 2. In other words, as the crystalline polycarbonate polyol, crystalline polycarbonate diol is particularly preferably used.

[0056] The polycarbonate polyol may contain a non-crystalline polycarbonate polyol as an optional component.

[0057] The amorphous polycarbonate polyol is a polycarbonate polyol that is liquid at 25° C. The term “liquid” means a state in which the viscosity at 25° C. measured by an E-type viscometer is 500,000 mPa·s or less.

[0058] Amorphous polycarbonate polyol can be obtained by modifying the above-mentioned crystalline polycarbonate polyol using a polyol as a modifier. As for the polyol as a modifier, for example, a divalent alcohol having 4 to 10 carbon atoms can be mentioned. As a divalent alcohol having 4 to 10 carbon atoms, for example, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, and 2,2-dimethyl-1,3-propanediol can be mentioned. They can be used alone or in combination of two or more.

[0059] It should be noted that the method for modifying the ring-opening polymer of ethylene carbonate using a dihydric alcohol is not particularly limited, and a known method can be used. For example, using a dihydric alcohol as an initiator, ethylene carbonate is subjected to ring-opening polymerization using a known method, and then the obtained ring-opening polymer is further copolymerized with a dihydric alcohol as a modifier.

[0060] The number average molecular weight (molecular weight calculated as polystyrene) of the amorphous polycarbonate polyol is greater than 400, preferably greater than 500, and more preferably greater than 1000. The number average molecular weight (molecular weight calculated as polystyrene) of the amorphous polycarbonate polyol is, for example, 10,000 or less, preferably 8,000 or less, more preferably 5,000 or less, further preferably 3,000 or less, and particularly preferably 2,000 or less.

[0061] The average hydroxyl number of the amorphous polycarbonate polyol is, for example, 1.8 or more, and preferably 2 or more. In addition, the average hydroxyl number of the amorphous polycarbonate polyol is, for example, 4 or less, preferably 3 or less, and more preferably 2 or less. The average hydroxyl number of the amorphous polycarbonate polyol is particularly preferably 2. In other words, as the amorphous polycarbonate polyol, amorphous polycarbonate diol is particularly preferably used.

[0062] The content ratio of the amorphous polycarbonate polyol relative to the total amount of the polycarbonate polyol (the total amount of the crystalline polycarbonate polyol and the amorphous polycarbonate polyol) is, for example, 50 mol% or less, preferably 40 mol% or less, more preferably 30 mol% or less, further preferably 20 mol% or less, further preferably 10 mol% or less, and particularly preferably 0 mol%.

[0063] In other words, the content ratio of the crystalline polycarbonate polyol relative to the total amount of the polycarbonate polyol (the total amount of the crystalline polycarbonate polyol and the amorphous polycarbonate polyol) is, for example, 50 mol% or more, preferably 60 mol% or more, more preferably 70 mol% or more, further preferably 80 mol% or more, further preferably 90 mol% or more, and particularly preferably 100 mol%. That is, the polycarbonate polyol is preferably composed of crystalline polycarbonate polyol.

[0064] The number average molecular weight (molecular weight calculated as polystyrene) of the polycarbonate polyol is greater than 400, preferably 500 or more, and more preferably 1000 or more. The number average molecular weight (molecular weight calculated as polystyrene) of the polycarbonate polyol is, for example, 10,000 or less, preferably 8,000 or less, more preferably 5,000 or less, further preferably 3,000 or less, and particularly preferably 2,000 or less.

[0065] The average hydroxyl number of the polycarbonate polyol is, for example, 1.8 or more, and preferably 2 or more. The average hydroxyl number of the polycarbonate polyol is, for example, 4 or less, preferably 3 or less, and more preferably 2 or less. The average hydroxyl number of the polycarbonate polyol is particularly preferably 2. In other words, as the polycarbonate polyol, polycarbonate diol is particularly preferably used.

[0066] The polycarbonate polyol can be used alone or in combination of two or more. It is preferred that two or more polycarbonate polyols be used in combination. That is, from the viewpoint of improving the expansion and contraction properties (restoration force), heat resistance and fingerprint recovery of the thermoplastic polyurethane resin with good balance, it is preferred that two or more polycarbonate polyols be used in combination.

[0067] More specifically, the polycarbonate polyol contains a first polycarbonate polyol having a number average molecular weight of 1,200 or less and a second polycarbonate polyol having a number average molecular weight of 1,800 or more.

[0068] As the first polycarbonate polyol, the above-mentioned crystalline polycarbonate polyol and the above-mentioned amorphous polycarbonate polyol can be mentioned. As the first polycarbonate polyol, from the viewpoint of improving the expansion and contraction characteristics (restoration force), heat resistance and fingerprint recovery of the thermoplastic polyurethane resin with good balance, the above-mentioned crystalline polycarbonate polyol can be preferably mentioned.

[0069] The number average molecular weight of the first polycarbonate polyol is greater than 400, preferably 500 or more, more preferably 1000 or more. The number average molecular weight of the first polycarbonate polyol is 1200 or less, preferably 1150 or less, more preferably 1100 or less, and further preferably 1050 or less.

[0070] As the second polycarbonate polyol, the above-mentioned crystalline polycarbonate polyol and the above-mentioned amorphous polycarbonate polyol can be mentioned. As the second polycarbonate polyol, from the viewpoint of improving the expansion and contraction characteristics (restoration force), heat resistance and fingerprint recovery of the thermoplastic polyurethane resin with good balance, the above-mentioned crystalline polycarbonate polyol can be preferably mentioned.

[0071] The number average molecular weight of the second polycarbonate polyol is 1800 or more, preferably 1850 or more, more preferably 1900 or more, and further preferably 1950 or more. The number average molecular weight (molecular weight in terms of polystyrene) of the second polycarbonate polyol is, for example, 10000 or less, preferably 8000 or less, more preferably 5000 or less, further preferably 3000 or less, and particularly preferably 2000 or less.

[0072] The polycarbonate polyol may contain, for example, only the first polycarbonate polyol. In addition, the polycarbonate polyol may contain, for example, only the second polycarbonate polyol. Preferably, the polycarbonate polyol contains the first polycarbonate polyol and the second polycarbonate polyol. When the polycarbonate polyol contains the first polycarbonate polyol and the second polycarbonate polyol, their content ratio can be appropriately set according to the purpose and use.

[0073] For example, relative to the total mole of the first polycarbonate polyol and the second polycarbonate polyol, the first polycarbonate polyol is, for example, greater than 0 mol%, preferably 40 mol% or more. In addition, relative to the total mole of the first polycarbonate polyol and the second polycarbonate polyol, the first polycarbonate polyol is, for example, less than 100 mol%, preferably 60 mol% or less.

[0074] In addition, relative to the total mole of the first polycarbonate polyol and the second polycarbonate polyol, the second polycarbonate polyol is, for example, greater than 0 mol%, preferably 40 mol% or more. In addition, relative to the total mole of the first polycarbonate polyol and the second polycarbonate polyol, the second polycarbonate polyol is, for example, less than 100 mol%, preferably 60 mol% or less.

[0075] The macropolyol may contain other macropolyols as optional components. Other macropolyols are macropolyols other than polycarbonate polyol.

[0076] Examples of other macromolecular polyols include polyether polyols, polyester polyols, polyurethane polyols, epoxy polyols, vegetable oil polyols, polyolefin polyols, acrylic polyols, and vinyl monomer-modified polyols, which may be used alone or in combination of two or more.

[0077] The content ratio of other macropolyols relative to the total amount of the macropolyol is, for example, 50 mass % or less, preferably 30 mass % or less, more preferably 10 mass % or less, and particularly preferably 0 mass %.

[0078] That is, the content ratio of the polycarbonate polyol relative to the total amount of the macropolyol is, for example, 50 mass % or more, preferably 70 mass % or more, more preferably 90 mass % or more, and particularly preferably 100 mass %. In other words, the macropolyol is particularly preferably composed of polycarbonate polyol.

[0079] The number average molecular weight (molecular weight in terms of polystyrene) of the macropolyol is greater than 400, preferably greater than 500, and more preferably greater than 1000. The number average molecular weight (molecular weight in terms of polystyrene) of the macropolyol is, for example, 10,000 or less, preferably 8,000 or less, more preferably 5,000 or less, further preferably 3,000 or less, and particularly preferably 2,000 or less.

[0080] The content ratio of the macromolecular polyol relative to the total amount of the macromolecular polyol and the low molecular weight polyol is, for example, 10 mol% or more, preferably 20 mol% or more, and more preferably 30 mol% or more. In addition, the content ratio of the macromolecular polyol relative to the total amount of the macromolecular polyol and the low molecular weight polyol is, for example, 95 mol% or less, preferably 70 mol% or less, and more preferably 50 mol% or less.

[0081] (2) Low molecular weight polyols

[0082] The low molecular weight polyol is an organic compound having two or more hydroxyl groups in the molecule and having a relatively low molecular weight. The term "relatively low molecular weight" means that the number average molecular weight is 400 or less.

[0083] The low molecular weight polyol includes, for example, a low molecular weight diol having carbon atoms of 2 to 6. The low molecular weight diol having carbon atoms of 2 to 6 is a compound having 2 to 6 carbon atoms in one molecule, two hydroxyl groups in one molecule, and a molecular weight of 400 or less.

[0084] As low molecular weight diols having 2 to 6 carbon atoms, for example, alkane diols having 2 to 6 carbon atoms, ether diols having 2 to 6 carbon atoms, and olefin diols having 2 to 6 carbon atoms can be mentioned. As alkane diols having 2 to 6 carbon atoms, for example, ethylene glycol, propylene glycol, 1,3-propylene glycol, 1,4-butanediol (1,4-BD), 1,3-butanediol, 1,2-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, and 2,2-dimethyl-1,3-propanediol can be mentioned. As ether diols having 2 to 6 carbon atoms, for example, diethylene glycol, triethylene glycol, and dipropylene glycol can be mentioned. As olefin diols having 2 to 6 carbon atoms, for example, 1,4-dihydroxy-2-butene can be mentioned. These can be used alone or in combination of two or more.

[0085] The carbon number of the low molecular weight diol having 2 to 6 carbon atoms is 2 or more, preferably 3 or more. The carbon number of the low molecular weight diol having 2 to 6 carbon atoms is 6 or less, preferably 5 or less.

[0086] The low molecular weight diol having 2 to 6 carbon atoms preferably has 4 carbon atoms.

[0087] As the low molecular weight diol having 2 to 6 carbon atoms, preferably, an alkane diol having 2 to 6 carbon atoms is used, and more preferably, 1,4-butanediol is used.

[0088] The low molecular weight polyol may contain other low molecular weight polyols as required. Other low molecular weight polyols are low molecular weight polyols other than low molecular weight diols having 2 to 6 carbon atoms. As other low molecular weight polyols, for example, low molecular weight diols having 7 or more carbon atoms and low molecular weight polyols having 3 valence or more may be cited. These may be used alone or in combination of two or more.

[0089] The content ratio of other low molecular weight polyols relative to the total amount of the low molecular weight polyols is, for example, 50 mass % or less, preferably 30 mass % or less, more preferably 10 mass % or less, particularly preferably 0 mass %.

[0090] That is, the content ratio of the low molecular weight diol having 2 to 6 carbon atoms relative to the total amount of the low molecular weight polyol is, for example, 50 mass % or more, preferably 70 mass % or more, more preferably 90 mass % or more, and particularly preferably 100 mass %. In other words, the low molecular weight polyol is particularly preferably composed of a low molecular weight diol having 2 to 6 carbon atoms.

[0091] The molecular weight of the low molecular weight polyol is, for example, 30 or more, preferably 70 or more. The molecular weight of the low molecular weight polyol is 400 or less, preferably 300 or less.

[0092] The content ratio of the low molecular weight polyol can be appropriately set according to the purpose and application. The content ratio of the low molecular weight polyol is preferably appropriately set so that the hard segment concentration described below is within a desired range.

[0093] For example, the content ratio of the low molecular weight polyol is, for example, 5 mol% or more, preferably 30 mol% or more, and more preferably 50 mol% or more, relative to the total amount of the macromolecular polyol and the low molecular weight polyol. In addition, the content ratio of the low molecular weight polyol is, for example, 90 mol% or less, preferably 80 mol% or less, and more preferably 70 mol% or less, relative to the total amount of the macromolecular polyol and the low molecular weight polyol.

[0094] 3. Thermoplastic polyurethane resin

[0095] As described above, the thermoplastic polyurethane resin is a reaction product of a polyisocyanate component and a polyol component as raw material components. In other words, the thermoplastic polyurethane resin can be produced by the reaction of a polyisocyanate component and a polyol component (reaction step).

[0096] In the reaction step, a known method can be adopted as a method for reacting the polyisocyanate component and the polyol component. Examples of the reaction method include a one-shot method and a prepolymer method.

[0097] In the one-shot method, for example, a polyisocyanate component and a polyol component are reacted at one time. In the prepolymer method, for example, first, a polyisocyanate component and a macromolecular polyol are reacted to synthesize an isocyanate-terminated prepolymer. Next, the isocyanate-terminated prepolymer is reacted with a low molecular weight polyol. From the viewpoint of improving various physical properties, the prepolymer method is preferably used.

[0098] In the prepolymer method, first, a polyisocyanate component and a macromolecular polyol are reacted to synthesize an isocyanate group-terminated prepolymer (prepolymer synthesis step).

[0099] In the prepolymer synthesis step, the polyisocyanate component and the macropolyol are mixed at a predetermined ratio. The mixing ratio is adjusted based on the equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group in the polyisocyanate component to the hydroxyl group in the macropolyol.

[0100] That is, the equivalent ratio of the isocyanate group in the polyisocyanate component to the hydroxyl group in the macropolyol (isocyanate group / hydroxyl group) is, for example, 1.3 or more, preferably 1.5 or more. In addition, the equivalent ratio of the isocyanate group in the polyisocyanate component to the hydroxyl group in the macropolyol (isocyanate group / hydroxyl group) is, for example, 20 or less, preferably 15 or less, more preferably 10 or less, and further preferably 8 or less.

[0101] When based on mass, the polyisocyanate component is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and more preferably 15 parts by mass or more, relative to 100 parts by mass of the macromolecular polyol. In addition, the polyisocyanate component is, for example, 150 parts by mass or less, preferably 100 parts by mass or less, and more preferably 90 parts by mass or less, relative to 100 parts by mass of the macromolecular polyol.

[0102] In the prepolymer synthesis step, the method for reacting the polyisocyanate component with the macropolyol is not particularly limited. Examples of the reaction method include bulk polymerization and solution polymerization.

[0103] In bulk polymerization, for example, a polyisocyanate component and a macromolecular polyol are reacted under a nitrogen stream. The reaction temperature is, for example, 50° C. or higher. In addition, the reaction temperature is, for example, 250° C. or lower, preferably 200° C. or lower. In addition, the reaction time is, for example, 0.5 hours or higher, preferably 1 hour or higher. In addition, the reaction time is, for example, 48 hours or lower, preferably 24 hours or lower.

[0104] In solution polymerization, a polyisocyanate component and a macromolecular polyol are reacted in the presence of a known organic solvent. The reaction temperature is, for example, 50° C. or higher. In addition, the reaction temperature is, for example, 120° C. or lower, preferably 100° C. or lower. In addition, the reaction time is, for example, 0.5 hours or higher, preferably 1 hour or higher. In addition, the reaction time is, for example, 48 hours or lower, preferably 24 hours or lower.

[0105] In this way, an isocyanate group-terminated prepolymer is obtained as a reaction product liquid of the polyisocyanate component and the macropolyol.

[0106] In the prepolymer synthesis step, a known urethanization catalyst may be added as needed. The mixing ratio of the urethanization catalyst may be appropriately set according to the purpose and application.

[0107] In the prepolymer synthesis step, the isocyanate group-terminated prepolymer may be purified by a known method as necessary. Examples of the purification method include distillation and extraction.

[0108] Next, in this method, the isocyanate group-terminated prepolymer is reacted with a low molecular weight polyol to obtain a thermoplastic polyurethane resin (chain extension step).

[0109] In the chain extension step, the isocyanate group-terminated prepolymer and the low molecular weight polyol are mixed at a predetermined ratio. The mixing ratio is adjusted based on the equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group in the isocyanate group-terminated prepolymer to the hydroxyl group in the low molecular weight polyol.

[0110] That is, the equivalent ratio of the isocyanate group in the isocyanate group-terminated prepolymer to the hydroxyl group in the low molecular weight polyol (isocyanate group / hydroxyl group) is, for example, 0.75 or more, preferably 0.9 or more. In addition, the equivalent ratio of the isocyanate group in the isocyanate group-terminated prepolymer to the hydroxyl group in the low molecular weight polyol (isocyanate group / hydroxyl group) is, for example, 1.3 or less, preferably 1.1 or less.

[0111] When the amount of the low molecular weight polyol is based on mass, the amount is, for example, 1.0 parts by mass or more, preferably 2.5 parts by mass or more, more preferably 3.5 parts by mass or more, further preferably 4.5 parts by mass or more, particularly preferably 5.5 parts by mass or more, and is, for example, 15.0 parts by mass or less, preferably 10.0 parts by mass or less, and more preferably 9.0 parts by mass or less, relative to 100 parts by mass of the isocyanate group-terminated prepolymer.

[0112] In the chain extension step, the method for reacting the isocyanate group-terminated prepolymer with the low molecular weight polyol is not particularly limited. Examples of the reaction method include the above-mentioned bulk polymerization and the above-mentioned solution polymerization.

[0113] Thus, a thermoplastic polyurethane resin is obtained as a reaction product of the isocyanate group-terminated prepolymer and the low molecular weight polyol.

[0114] In addition, in the chain extension step, a known urethanization catalyst may be blended as necessary. The blending ratio of the urethanization catalyst may be appropriately set according to the purpose and application.

[0115] Thermoplastic polyurethane resin can contain known additives as required. As additives, for example, antioxidants, heat stabilizers, ultraviolet light absorbers, light stabilizers, and anti-hydrolysis agents, dyes, plasticizers, anti-blocking agents, surface modifiers, lubricants, mold release agents, pigments, fillers, rust inhibitors, and fillers can be cited. They can be used alone or in combination of two or more. The amount of additives added and the time of addition can be appropriately set according to the purpose and use.

[0116] The thermoplastic polyurethane resin may be subjected to an aging treatment (aging step) as required. In the aging step, the above-mentioned thermoplastic polyurethane resin (unaged product) is subjected to an aging treatment. Thus, an aged product of the thermoplastic polyurethane resin is obtained.

[0117] The aging temperature is, for example, 50° C. or more, preferably 60° C. or more, and more preferably 70° C. or more. In addition, the aging temperature is, for example, 100° C. or less, and preferably 90° C. or less. The aging time is, for example, 3 days or more, preferably 4 days or more, more preferably 5 days or more, and further preferably 6 days or more. In addition, the aging time is, for example, 10 days or less, preferably 9 days or less, and more preferably 8 days or less.

[0118] From the viewpoint of heat resistance, the hard segment concentration of the thermoplastic polyurethane resin is, for example, 18 mass % or more, preferably 20 mass % or more, and more preferably 22 mass % or more.

[0119] From the viewpoint of expansion and contraction characteristics, the hard segment concentration of the thermoplastic polyurethane resin is, for example, 35 mass % or less, preferably 30 mass % or less, and more preferably 25 mass % or less.

[0120] When the hard segment concentration of the thermoplastic polyurethane resin is within the above range, fingerprint recovery property and heat resistance can be achieved particularly well at the same time.

[0121] That is, in the above-mentioned thermoplastic polyurethane resin, the polyisocyanate component contains 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane. The crystallinity of 1,3-bis(isocyanate methyl)cyclohexane is lower than that of 1,4-bis(isocyanate methyl)cyclohexane. Therefore, in the case where the polyisocyanate component contains 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane, the crystallinity of the thermoplastic polyurethane resin becomes relatively low compared to the case where the polyisocyanate component contains only 1,4-bis(isocyanate methyl)cyclohexane. As a result, the thermoplastic polyurethane resin has excellent fingerprint recovery. On the other hand, in the case where the crystallinity of the thermoplastic polyurethane resin is relatively low, the heat resistance of the thermoplastic polyurethane resin sometimes becomes low. In such a case, if the hard segment concentration is adjusted to a specified range, the reduction in the heat resistance of the thermoplastic polyurethane resin can be suppressed. That is, when the hard segment concentration is within the above range, the thermoplastic polyurethane resin can achieve both fingerprint recovery property and heat resistance particularly well.

[0122] The concentration of the hard segment (the hard segment formed by the reaction of the polyisocyanate component and the low molecular weight polyol) of the thermoplastic polyurethane resin can be calculated by a known method based on the mixing ratio (charge) of each component, for example.

[0123] More specifically, for example, when the prepolymer method is used, the hard segment concentration can be calculated from the following formula based on the blending formula (charge) of each component.

[0124] [Low molecular weight polyol (g) + (Low molecular weight polyol (g) / Molecular weight of low molecular weight polyol (g / mol)) × Average molecular weight of polyisocyanate component (g / mol)] ÷ (Polyisocyanate component (g) + Total mass of polyol component (g)) × 100

[0125] The raw material components of the thermoplastic polyurethane resin include 1,4-bis(isocyanatemethyl)cyclohexane, a crystalline polycarbonate polyol, and a polyol component including a low molecular weight polyol at predetermined ratios.

[0126] 1,4-bis(isocyanatomethyl)cyclohexane has relatively high crystallinity. In addition, the low molecular weight polyol forms a hard segment, thereby improving crystallinity. In addition, the crystalline polycarbonate polyol has relatively high crystallinity.

[0127] In addition, the raw material component contains 1,3-bis(isocyanatemethyl)cyclohexane. 1,3-bis(isocyanatemethyl)cyclohexane has relatively low crystallinity.

[0128] In addition, among the raw material components, the ratio of 1,4-bis(isocyanatemethyl)cyclohexane to 1,3-bis(isocyanatemethyl)cyclohexane is adjusted to be within a predetermined range.

[0129] That is, the crystallinity of the polyurethane structure is adjusted by the raw material components. As a result, the thermoplastic polyurethane resin has a good balance of stretching characteristics (restoring force), heat resistance and fingerprint recovery.

[0130] Furthermore, when the crystallinity of the polyurethane structure is adjusted as described above, the thermoplastic polyurethane resin also has excellent blooming resistance and melting characteristics.

[0131] Therefore, the thermoplastic polyurethane resin can be suitably used in the production of various molded products. That is, the thermoplastic polyurethane resin can be molded by a known molding method to obtain a molded product containing the thermoplastic polyurethane resin.

[0132] Examples of the molding method include heat compression molding, injection molding, extrusion molding, cutting molding, melt spinning molding, and 3D printer molding, which may be used alone or in combination of two or more.

[0133] As a molding method, extrusion molding is preferably mentioned. In extrusion molding, for example, first, a thermoplastic polyurethane resin is molded once to obtain pellets of the thermoplastic polyurethane resin.

[0134] Next, the pellets of the thermoplastic polyurethane resin are subjected to secondary molding to obtain a molded article of a desired shape.

[0135] As the shape of the molded product, for example, a film, a sheet, a plate, a fiber, a wire bundle, a tubular, a hollow, and a box-like shape can be enumerated. They can be used alone or in combination of two or more. As the shape of the molded product, a film can be preferably enumerated.

[0136] In other words, as the molded article, preferably, there is a film containing a thermoplastic polyurethane resin. Such a film contains the above-mentioned thermoplastic polyurethane resin, and therefore has both fingerprint recovery, stretching characteristics (restoration force), and heat resistance in a good balance.

[0137] Therefore, the above-mentioned film can be suitably used in the field requiring the above-mentioned various physical properties. More specifically, the above-mentioned film can be suitably used as a base film of various protective films, for example. As the protective film, there is no particular limitation, for example, a paint protection film (PPF), a protective film of an automobile interior decoration material, a protective film of a wind power generation blade, and a protective film of glass can be cited. Preferably, a paint protection film can be cited. The paint protection film can be used to protect the painted surface of various products in various industrial fields such as the automobile industry.

[0138] More specifically, paint protection films (PPF) can be attached to the painted surfaces of various products (for example, automobiles and motorcycles), thereby protecting the surfaces of various products.

[0139] The coating protection film (PPF) at least comprises a film containing the above-mentioned thermoplastic polyurethane resin. For example, the coating protection film (PPF) is a laminated film, which comprises a peeling layer, an adhesive layer disposed on at least one surface of the peeling layer, and a base film layer disposed on at least one surface of the adhesive layer. More specifically, the coating protection film (PPF) comprises, for example, a peeling layer containing a polyester resin, an acrylic adhesive layer disposed on the peeling layer, and a base film layer disposed on the acrylic adhesive layer. In addition, the coating protection film (PPF) may also further comprise a surface protection layer disposed on the base film layer.

[0140] Moreover, the base film layer contains the above-mentioned film. That is, as the base film layer of the coating protection film (PPF), a film containing the above-mentioned thermoplastic polyurethane resin can be used. As a result, the coating protection film (PPF) has excellent expansion and contraction properties (restoration force), heat resistance and fingerprint recovery. Therefore, the coating protection film (PPF) can well protect various products (automobiles, motorcycles, etc.).

[0141] In addition, the above-mentioned film (for example, the base film layer) can be colored by any method. That is, the above-mentioned film (for example, the base film layer) can also be a color film. For example, in the case where the base film layer of the protective film is a color film, the protective film can protect various products as described above and color the various products. More specifically, for example, in the case where the base film of the paint protection film for automobiles is a color film, the paint protection film can protect the painted surface of the automobile and easily change the color of the automobile body.

[0142] The thermoplastic polyurethane resin, film and coating protection film can be suitably used in various industrial fields requiring stretching characteristics (restoring force), heat resistance and fingerprint recovery. In particular, the thermoplastic polyurethane resin, film and coating protection film can be suitably used in the field of coating protection for protecting the painted surface of vehicles (e.g., automobiles and motorcycles).

[0143] Example

[0144] Next, the present invention is described based on embodiments and comparative examples, but the present invention is not limited by them. It should be noted that, unless otherwise specified, "parts" and "%" are based on mass. In addition, the specific numerical values ​​such as the mixing ratio (containing ratio), physical property values, and parameters used in the following description can be replaced by the upper limit value (numerical value defined in the form of "below", "less than") or the lower limit value (numerical value defined in the form of "above", "greater than") recorded in the above-mentioned "specific embodiments" and corresponding to the mixing ratio (containing ratio), physical property values, and parameters.

[0145] 1) Raw materials

[0146] <Polyisocyanate component (a)>

[0147] 1,4-H6XDI: 1,4-bis(isocyanatemethyl)cyclohexane obtained according to the description of Production Example 3 of International Publication No. 2019 / 069802. The trans isomer is 86 mol% and the cis isomer is 14 mol%.

[0148] 1,3-H6XDI: 1,3-bis(isocyanatomethyl)cyclohexane, trade name TAKEN ATE 600, manufactured by Mitsui Chemicals

[0149] <Macropolyol (b)>

[0150] b-1) PCD1000: number average molecular weight (Mn) 1000, crystalline polycarbonate diol, trade name ETERNACOLLUH-100W, average hydroxyl number 2, manufactured by Ube Industries

[0151] b-2) PCD2000: number average molecular weight (Mn) 2000, crystalline polycarbonate diol, trade name ETERNACOLLUH-200W, average hydroxyl number 2, manufactured by Ube Industries

[0152] b-3) Liquid PCD1000: number average molecular weight (Mn) 1000, amorphous polycarbonate diol, trade name ETERNACOLL UP-100, average hydroxyl number 2, manufactured by Ube Industries

[0153] b-4) Liquid PCD2000: number average molecular weight (Mn) 2000, amorphous polycarbonate diol, trade name ETERNACOLL UP-200, average hydroxyl number 2, manufactured by Ube Industries

[0154] b-5) PCL1000: number average molecular weight (Mn) 1000, polycaprolactone diol, trade name Placcel 210N, average hydroxyl number 2, manufactured by Daicel

[0155] b-6) PCL2000: number average molecular weight (Mn) 2000, polycaprolactone diol, trade name Placcel 220N, average hydroxyl number 2, manufactured by Daicel

[0156] <Low molecular weight polyol (c)>

[0157] 1,4-BD: 1,4-butanediol, manufactured by Mitsubishi Chemical Corporation

[0158] 2) Thermoplastic polyurethane resin

[0159] Examples 1 to 14 and Comparative Examples 1 to 14

[0160] According to the formulations described in Tables 1 to 4, thermoplastic polyurethane resins and sheets were obtained.

[0161] More specifically, first, the measurement was performed on a macropolyol (b) whose temperature was previously adjusted to 80° C. The macropolyol (b) was stirred for 1 hour in an oil bath at 80° C. under a nitrogen atmosphere. Next, the following additives were added to the macropolyol (b), and the mixture was stirred for 1 hour in an oil bath at 80° C. under a nitrogen atmosphere.

[0162] Irganox 245 (heat-resistant stabilizer manufactured by BASF) 0.3 parts by mass

[0163] Tinuvin 571 (UV absorber manufactured by BASF) 0.4 parts by mass

[0164] ADK STAB LA-72 (HALS manufactured by ADEKA Corporation) 0.1 parts by mass

[0165] (The above is a ratio relative to 100 parts by mass of the total amount of the polyisocyanate component, the macromolecular polyol and the low molecular weight polyol)

[0166] Next, the polyisocyanate component (a) was added to the mixture of the macromolecular polyol (b) and the additives in the proportions listed in Tables 1 to 4. A solution of tin octylate (solvent: diisononyl adipate, concentration: 4% by mass) was further added as a urethanization catalyst in a proportion of 5 ppm relative to the mixture. Next, the mixture was stirred and mixed in an oil bath at 80° C. for 5 minutes to react. Thus, an isocyanate-terminated prepolymer was obtained (prepolymer synthesis step).

[0167] Next, the low molecular weight polyol (c) whose temperature was adjusted to 80° C. was added to the isocyanate group-terminated prepolymer, and the mixture was stirred and mixed for 3 to 20 minutes.

[0168] The amount of low molecular weight polyol (c) added was adjusted so that the equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group in the isocyanate group-terminated prepolymer to the hydroxyl group in the low molecular weight polyol (c) was 1.00. The above-mentioned tin octylate solution was appropriately added while observing the heat release rate.

[0169] Next, the reaction product liquid was poured into a Teflon (registered trademark) barrel adjusted to 150°C, and reacted at 150°C for 2 hours and further at 100°C for 20 hours (chain extension step). Thus, a thermoplastic polyurethane resin was obtained.

[0170] Next, the thermoplastic polyurethane resin (unaged product) was taken out and cut into dice using a rubber cutter. Next, the dice-shaped thermoplastic polyurethane resin was crushed using a crusher. Thus, crushed pellets were obtained.

[0171] Next, the crushed pellets were aged in an oven at 80° C. for 7 days and dried at 23° C. for 12 hours under vacuum. Thus, an aged product of a thermoplastic polyurethane resin was obtained.

[0172] Then, the aged product of the thermoplastic polyurethane resin was molded using a single screw extruder (model: SZW40-28MG, manufactured by TECHNOVE L) to obtain pellets (primary molded product). It should be noted that the screw speed of the extruder was 30 rpm and the barrel temperature was 150° C. to 250° C. The pellets of the thermoplastic polyurethane resin were dried at 80° C. for 12 hours under vacuum.

[0173] The pellets were then molded into a film (secondary molded product) using a single screw extruder (model: SZW40-28MG, manufactured by TECHNOVE L). The screw speed of the extruder was 20 rpm and the barrel temperature was 150° C. to 250° C. The thermoplastic polyurethane resin film was used in the following evaluation test.

[0174] In addition, the hard segment concentration of the thermoplastic polyurethane resin was calculated by the following formula: [low molecular weight polyol (g) + (low molecular weight polyol (g) / molecular weight of low molecular weight polyol (g / mol)) × average molecular weight of polyisocyanate component (g / mol)] ÷ (polyisocyanate component (g) + total mass of polyol component (g)) × 100

[0175] 4) Evaluation

[0176] <Hardness (Shore A)>

[0177] The Shore A hardness of the thermoplastic polyurethane resin film was measured in accordance with JIS K 7312 (1996).

[0178] <Stretching properties: recovery rate (shape recovery rate)>

[0179] A thermoplastic polyurethane resin film was placed on a universal testing machine Model 205N (manufactured by INTESCO, with a distance between markings of 80 mm and a tensile speed of 500 ml / min), stretched to 60% (48 mm) of the distance between markings, and then released.

[0180] 15 seconds after release, the distance between the marking lines is measured to determine the recovery rate of the film. It should be noted that the recovery rate of the film is the ratio (%) of the length of the film before elongation to the length of the film after elongation. The higher the recovery rate of the film (close to 100%), the higher the recovery rate (shape recovery rate).

[0181] The criteria for determining the expansion and contraction characteristics are described below.

[0182] ◎: Recovery rate is more than 98.5%

[0183] ○: Recovery rate is 97.5% or more and less than 98.5%

[0184] △: Recovery rate is 97.0% or more and less than 97.5%

[0185] ×: Recovery rate is less than 97.0%

[0186] <Fingerprint recovery>

[0187] A center punch with a diameter of 20 mm was placed against the surface of the thermoplastic polyurethane resin film, and the punch was pushed out 14 mm toward the film to deform it convexly. The film was then released from the punch. After 10 minutes, the height of the convex portion (punch mark) of the film was measured.

[0188] In addition, the convex portion remaining rate of the film was calculated. The convex portion remaining rate is the ratio (%) of the height of the convex portion after release to the height of the convex portion before release. The lower the convex portion remaining rate (closer to 0%), the higher the fingerprint restoration.

[0189] The following describes the criteria for determining fingerprint recovery.

[0190] ◎: The convex part remaining rate is less than 10%

[0191] ○: The convex portion remaining rate is 10% or more and less than 17%

[0192] △: The convex portion remaining ratio is 17% or more and less than 19%

[0193] ×: The convex portion remaining rate is 19% or more

[0194] <Heat resistance: Storage elastic modulus (E')>

[0195] The dynamic viscoelasticity spectrum of the thermoplastic polyurethane resin film was measured using a dynamic viscoelasticity measuring apparatus (manufactured by IT Sokuryo Seigyo Co., Ltd., model: DVA-220) under the conditions of a measuring temperature of -100°C to 250°C, a heating rate of 5°C / min, a tensile mode, a length between markings of 20 mm, a static / dynamic stress ratio of 1.8, and a measuring frequency of 10 Hz.

[0196] Then, the storage elastic modulus E' was measured at 80° C. The higher the E', the better the heat resistance.

[0197] The criteria for judging heat resistance are described below.

[0198] ◎: Storage elastic modulus E' (80℃) is 20×10 6 MPa or above

[0199] ○: Storage elastic modulus E' (80°C) is 10×10 6 MPa or more and less than 20×10 6 MPa

[0200] ×: Storage elastic modulus E' (80°C) less than 10×10 6 MPa

[0201] <Bloom resistance>

[0202] The film of the thermoplastic polyurethane resin was stored at 30° C. and a relative humidity of 80% for 35 days. Then, the haze of the film was measured using a HAZE METER NDH-5000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0203] <Melting enthalpy (unit: J / g)>

[0204] The measurement was performed as follows using a differential scanning calorimeter (DSC7000X, manufactured by Hitachi High-Tech Science).

[0205] That is, about 10 mg of thermoplastic polyurethane resin was collected in an aluminum dish, and the aluminum dish was covered with a lid and crimped to obtain a product to be used as a test sample. A product obtained by collecting aluminum oxide in the same manner was used as a reference sample.

[0206] After setting the sample and reference at the specified positions in the chamber (cell), the sample was cooled from 20°C to -100°C at a rate of 10°C / min under a nitrogen flow of 30NmL / min. After maintaining this temperature for 5 minutes, the temperature was increased to 270°C at a rate of 10°C / min, and then cooled to -70°C at a rate of 10°C / min.

[0207] Then, among the peaks appearing during the temperature rise from -100°C to 270°C, the peak temperature of the endothermic peak (melting peak) at 160°C or higher and the calorific value (enthalpy change) (J / g) of the peak were measured.

[0208] [Table 1]

[0209]

[0210] [Table 2]

[0211]

[0212] [Table 3]

[0213]

[0214] [Table 4]

[0215]

[0216] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and is not to be construed as limiting. Modifications of the present invention that are obvious to those skilled in the art are included in the appended claims.

[0217] Industrial Applicability

[0218] The thermoplastic polyurethane resin, film, and paint protection film of the present invention can be suitably used in the field of paint protection for protecting the painted surface of a vehicle.

Claims

1. A thermoplastic polyurethane resin comprising a reaction product of a polyisocyanate component and a polyol component, The polyisocyanate component comprises 1,4-bis(isocyanate methyl)cyclohexane and 1,3-bis(isocyanate methyl)cyclohexane, The polyol component comprises polycarbonate polyol and low molecular weight polyol, The polycarbonate polyol includes a crystalline polycarbonate polyol that is solid at 25° C. Relative to the total amount of 1,4-bis(isocyanatemethyl)cyclohexane and 1,3-bis(isocyanatemethyl)cyclohexane, The ratio of 1,4-bis(isocyanatemethyl)cyclohexane is 50 mol% to 90 mol%, The ratio of 1,3-bis(isocyanatemethyl)cyclohexane is 10 mol% to 50 mol%.

2. The thermoplastic polyurethane resin according to claim 1, wherein The polycarbonate polyol is composed of the crystalline polycarbonate polyol.

3. The thermoplastic polyurethane resin according to claim 1, wherein The thermoplastic polyurethane resin has a hard segment concentration of 18% by mass or more and 35% by mass or less.

4. The thermoplastic polyurethane resin according to claim 1, wherein The polycarbonate polyol comprises: a first polycarbonate polyol having a number average molecular weight of 1200 or less, and A second polycarbonate polyol having a number average molecular weight of 1800 or more.

5. A membrane, characterized in that The invention comprises the thermoplastic polyurethane resin according to claim 1.

6. A coating protective film having: Peel layer, an adhesive layer disposed on at least one surface of the release layer, and a base film layer disposed on at least one surface of the adhesive layer, The base film layer contains the film according to claim 5.

Citation Information

Patent Citations

  • Polyurethane resin

    WO2009051114A1

  • Polyurethane resin, molded article, and method for producing polyurethane resin

    WO2019069802A1