Electrolytic capacitor

By using glycol ether as liquid components in the electrolytic capacitor, the problem of degradation of electrostatic capacitance performance in the low temperature environment is solved, and good capacitance and low temperature characteristics are improved below -50°C.

CN118974864APending Publication Date: 2024-11-15PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031251.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The electrostatic capacitance performance of existing electrolytic capacitors deteriorates in low temperature environments, making it difficult to maintain good capacitance, especially at temperatures below -50°C.

Method used

An electrolytic capacitor containing glycol ether as a liquid component is used. The glycol ether has a -(CH2O)n-structure, and n is an integer of 1 or more. It is used to improve the low temperature characteristics of the electrolytic capacitor, by using monoalkyl ether and dialkyl. As a solvent, the content of the mixture of ethers is preferably higher than 50% in order to reduce viscosity and maintain good ionic conductivity.

Benefits of technology

Even at low temperatures below minus 50°C, the electrolytic capacitor can maintain good electrostatic capacitance, reduce the equivalent series resistance (ESR) and dielectric loss tangent (tanδ), and improve the overall low-temperature characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974864A_ABST
    Figure CN118974864A_ABST
Patent Text Reader

Abstract

An electrolytic capacitor provided with a capacitor element provided with an anode body having a dielectric layer and a solid electrolyte in contact with the dielectric layer, and a liquid component containing a solvent and a solute, the solvent containing a glycol ether as a first component, and the solute containing a glycol ether as a second component. The glycol ether contains at least one selected from the group consisting of monoalkyl ethers and dialkyl ethers, the glycol ether has a 1 (CH2O) n-structure, and n is an integer of 1 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to electrolytic capacitors. Background Art

[0002] As a small-sized, large-capacity, low-ESR (equivalent series resistance) capacitor, a hybrid electrolytic capacitor having a solid electrolyte and a liquid component is considered promising.

[0003] Patent Document 1 proposes that a capacitor element of a solid electrolytic capacitor contains polyethylene glycol and (-CH2-CH(R)-O-) n A compound with a chemical structure of (wherein R represents an alkyl group having 1 to 4 carbon atoms and n represents an integer).

[0004] Patent Document 2 proposes an electrolytic solution for an electrolytic capacitor in which an organic carboxylate is dissolved in a mixed solvent containing γ-butyrolactone and ethylene glycol ether or diethylene glycol ether.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2017-27992

[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 62-1218 Summary of the invention

[0009] Problems to be solved by the invention

[0010] Electrolytic capacitors are used in various temperature environments. On the other hand, liquid components are easily affected by temperature changes. Among them, it is important to maintain the low-temperature characteristics of electrolytic capacitors. In many applications, electrolytic capacitors that can maintain electrostatic capacitance even at low temperatures (e.g., below -50°C) are required.

[0011] Means for solving problems

[0012] One aspect of the present invention relates to an electrolytic capacitor comprising a capacitor element and a liquid component, wherein the capacitor element comprises an anode body having a dielectric layer and a solid electrolyte in contact with the dielectric layer, wherein the liquid component comprises a solvent and a solute, wherein the solvent comprises a glycol ether as a first component, wherein the glycol ether comprises at least one selected from a monoalkyl ether and a dialkyl ether, and wherein the glycol ether has -(CH2O) n -structure, and n is an integer greater than 1.

[0013] Effects of the Invention

[0014] According to the present invention, it is possible to provide an electrolytic capacitor including a liquid component that can maintain good electrostatic capacitance even at low temperatures.

[0015] The novel features of the present invention are described in the appended claims, but both the configuration and content of the present invention, together with other objects and features of the present invention, will be better understood through the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic cross-sectional view of an electrolytic capacitor according to one embodiment of the present invention.

[0017] Figure 2 It is a schematic diagram for explaining the structure of the capacitor element of the same embodiment. DETAILED DESCRIPTION

[0018] The following describes an electrolytic capacitor according to an embodiment of the present invention, but the electrolytic capacitor of the present invention is not limited to the following embodiments. In the following description, specific values ​​and materials are sometimes exemplified, but other values ​​and materials may also be applied as long as the effects of the present invention can be obtained. In this specification, a description such as "value A to value B" includes value A and value B, and can be replaced by "value A or more and value B or less".

[0019] In the following description, when the lower limit and upper limit of the numerical value related to a specific physical property, condition, etc. are illustrated, as long as the lower limit is not above the upper limit, any one of the illustrated lower limits and any one of the illustrated upper limits can be arbitrarily combined. When multiple materials are illustrated, as long as there is no special mention, one can be selected from them and used alone, or two or more can be used in combination.

[0020] In the following description, the term “comprising” or “including” includes “comprising (or including)”, “consisting essentially of” and “consisting of”.

[0021] In the following description, "electrolytic capacitor" may be replaced by "solid electrolytic capacitor" or "hybrid electrolytic capacitor". In addition, "capacitor" may be replaced by "capacitor". In addition, "liquid component" may be replaced by "electrolyte" in some cases.

[0022] An electrolytic capacitor according to one embodiment of the present invention comprises a capacitor element and a liquid component. The capacitor element comprises an anode body having a dielectric layer. The shape of the anode body is not particularly limited. The anode body can be formed, for example, of a metal foil or a porous metal sintered body. The surface portion of the metal foil can have a porous portion. For example, the surface portion of the metal foil can be roughened by etching. The capacitor element can have a cathode portion.

[0023] The cathode portion includes, for example, a solid electrolyte in contact with the dielectric layer. The solid electrolyte may be a conductive polymer, a conductive inorganic material (such as manganese dioxide), a TCNQ complex salt, or the like.

[0024] The liquid component includes a solvent and a solute. The solvent includes a glycol ether as a first component. The glycol ether includes at least one selected from a monoalkyl ether and a dialkyl ether (hereinafter, also referred to as "glycol ether (G)"). In addition, the glycol ether (G) has -(CH2O) n -structure, and n is an integer greater than 1.

[0025] That is, the monoalkyl ether has an alkyl group at one end, an OH group at the other end, and a main structural group between the alkyl and OH groups. In addition, the dialkyl ether has alkyl groups at both ends, and a main structural group between the two alkyl groups. The main structural group has oxyethylene or polyoxyethylene.

[0026] Monoalkyl ethers, for example, have R-(CH2O) n -OH. Dialkyl ethers, for example, have R-(CH2O) n -R. The two R's in the dialkyl ether molecule may be the same or different. The glycol ether (G) may be a mixture of a plurality of molecules having different n's or different R's.

[0027] Unlike diol compounds having two OH groups, diol ethers (G) have only one OH group or no OH group at all. Therefore, diol ethers (G) are less susceptible to temperature changes than diol compounds. By using a liquid component containing diol ethers (G), an electrolytic capacitor that can maintain good electrostatic capacitance even at a low temperature of minus 50°C or below can be obtained.

[0028] The glycol ether (G) is preferably liquid at room temperature (25° C.), and preferably has a melting point of at least 0° C. or lower.

[0029] In addition, by using glycol ether (G), it is easy to maintain low ESR and dielectric loss tangent (tanδ) at low temperatures, for example, below -50°C. This is considered to be related to the ability to well maintain the ion conductivity of the liquid component at low temperatures. That is, it is considered that by using glycol ether (G), the low-temperature characteristics of the electrolytic capacitor, for example, below -50°C, are improved overall.

[0030] It should be noted that the main structural group of glycol ether (G) can be composed of only oxyethylene or polyoxyethylene, or it can have oxyalkylene groups other than oxyethylene. Wherein, more than 60% by mass of the main structural group, and then more than 80% by mass (can also be 100%), is composed of oxyethylene or polyoxyethylene. It can be considered that oxyethylene, compared with other oxyalkylene groups, contributes to improving ionic conductivity, and has low volatility, which is conducive to the improvement of low temperature characteristics at this point. It can be considered that the more the ratio of oxygen in the main structural group relative to carbon, the more ionic conductivity is improved, which is more conducive to high capacity.

[0031] Compared with diol compounds, diol ethers (G) have a lower probability of forming hydrogen bonds and are less likely to undergo esterification reactions. Therefore, it is believed that diol ethers (G) are less susceptible to temperature changes than diol compounds. Among them, it is believed that the formation of hydrogen bonds is the main reason for increasing the viscosity of the liquid component at low temperatures and reducing the ion conductivity of the liquid component.

[0032] It can be considered that the dialkyl ether having no OH group at all is less susceptible to temperature changes than the monoalkyl ether having 1 OH group. On the other hand, it can be considered that the monoalkyl ether having 1 OH group is difficult to penetrate the sealing member compared with the dialkyl ether, and therefore has the effect of greatly suppressing the evaporation of the liquid component of the electrolytic capacitor. From the viewpoint of obtaining better low-temperature characteristics, the content of the dialkyl ether in the glycol ether (G) is preferably more than 50% by mass, and more than 90% by mass can be dialkyl ether. From the viewpoint of obtaining good low-temperature characteristics and suppressing the evaporation of the liquid component, the content of the monoalkyl ether in the glycol ether (G) can be set to more than 10% by mass, and further set to more than 20% by mass.

[0033] In the structure -(CH2O) n -, n can be 1 or more, and the average value of n can be, for example, 3 or more, 4 or more, or 5 or more. The average value of n can be, for example, 20 or less, 15 or less, or 10 or less. If the n value is within such a range, the viscosity of the liquid component containing the glycol ether (G) can be maintained lower. In addition, better ion conductivity of the liquid component can be maintained. Among them, it is preferred that 90% by mass or more of the glycol ether have an integer n in the range of 1 or more and 11 or less.

[0034] From the viewpoint of ensuring sufficient ion conductivity, the alkyl group (e.g., R—(CH 2 O)) of the glycol ether (G) n -OH and R-(CH2O) n-R) is preferably a C1-C10 alkyl group having 1 to 10 carbon atoms. Here, "Cn1-Cn2 alkyl" is a general term for alkyl groups having n1 (n1 is an integer) to n2 (n2 is an integer greater than n1) carbon atoms. For example, "C1-C3 alkyl" refers to at least one selected from methyl, ethyl, n-propyl and isopropyl. Alkyl (R) can be a C1-C5 alkyl group or a C1-C3 alkyl group.

[0035] 90 mol% or more of the alkyl groups in the glycol ether (G) may be C1-C10 alkyl groups. For example, when the content of glycol ether (G) in the liquid component of a certain electrolytic capacitor is x1 mol, y mol% of glycol ether (G) is dialkyl ether, and (100-y) mol% is monoalkyl ether, the liquid component contains (2×x1×y / 100)+(x1×(1-y / 100)) mol of alkyl groups. In this case, 0.9×{(2×x1×y / 100)+(x1×(1-y / 100))} mol or more may be C1-C10 alkyl groups, C1-C5 alkyl groups, or C1-C3 alkyl groups.

[0036] Similarly, 90 mol% or more of the alkyl groups of the monoalkyl ether in the glycol ether (G) may be C1-C10 alkyl groups, C1-C5 alkyl groups, or C1-C3 alkyl groups.

[0037] Similarly, 90 mol% or more of the alkyl groups in the dialkyl ether may independently be C1-C10 alkyl groups, C1-C5 alkyl groups, or C1-C3 alkyl groups.

[0038] The number average molecular weight Mn of the glycol ether (G) can be, for example, 100 or more, 150 or more, or 200 or more. The number average molecular weight Mn can be, for example, 4000 or less, 2000 or less, or 1000 or less. If the number average molecular weight Mn is within such a range, the viscosity of the liquid component containing the glycol ether (G) can be maintained lower. In addition, better ion conductivity of the liquid component can be maintained. Among them, the number average molecular weight of the glycol ether is preferably 100 or more and 1000 or less.

[0039] As a solvent, only glycol ether (G) may be used, or components other than glycol ether (G) may be used. However, from the viewpoint of obtaining a better electrostatic capacitance at a low temperature of minus 50° C. or less, the content of glycol ether (G) in the liquid component may be 10% by mass or more, 15% by mass or more, or 20% by mass or more. The content of glycol ether (G) in the liquid component may be 95% by mass or less, 90% by mass or less, or 70% by mass or less.

[0040] The solvent preferably contains at least one selected from ethylene glycol and sulfolane (hereinafter also referred to as “second component”) as a component other than the glycol ether (G).

[0041] Ethylene glycol is not easy to penetrate the sealing member even at high temperature, so it is considered to have the effect of suppressing the evaporation of the liquid component of the electrolytic capacitor. In addition, when a conductive polymer is used as a solid electrolyte, it is considered that ethylene glycol has the effect of improving the crystallinity of the conductive polymer and thus improving the conductivity. In addition, ethylene glycol has excellent thermal conductivity and excellent heat dissipation when a pulsating current is generated.

[0042] Sulfolane is stable at high temperatures and can contribute to lowering the viscosity of the liquid component. Sulfolane can solidify at low temperatures, but by using it in combination with the glycol ether (G), this phenomenon can be suppressed and the advantages of sulfolane can be enjoyed.

[0043] The content of the second component in the liquid component may be, for example, 5% by mass or more, or 20% by mass or more. The content of the second component in the liquid component may be, for example, 90% by mass or less, or 60% by mass or less.

[0044] The solvent may further contain γ-butyrolactone (hereinafter also referred to as "third component") as a component other than the glycol ether (G). γ-Butyrolactone is stable in a wide temperature range and has a low viscosity. The content of the third component in the liquid component may be, for example, 5% by mass or more, or 20% by mass or more. The content of the third component in the liquid component may be, for example, 70% by mass or less, or 50% by mass or less.

[0045] In addition to the components already described, the solvent may also contain a fourth component. The content of the fourth component in the liquid component is preferably limited to 20% by mass or less. As the fourth component, for example, diol compounds other than ethylene glycol, sulfone compounds other than cyclopentane sulfone, lactone compounds other than γ-butyrolactone, and carbonate compounds may be cited. As diol compounds, for example, propylene glycol, trimethylene glycol, 1,4-butanediol, pentanediol, and hexanediol may be cited. As sulfone compounds, for example, chain sulfones (dimethyl sulfone, diethyl sulfone, etc.), cyclic sulfones (3-methylcyclopentane sulfone, 3,4-dimethylcyclopentane sulfone, 3,4-dibenzylcyclopentane sulfone, etc.) may be cited. As lactone compounds, for example, γ-valerolactone may be cited. As carbonate compounds, for example, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, and fluoroethylene carbonate may be cited. The fourth component may be used alone or in combination of two or more.

[0046] When the first component and the second component are used in combination, it is preferred to use them in consideration of the distribution so that each can exert the described characteristics. For example, the mass of the first component can be more than 0.1 times and less than 5 times the mass of the second component, or more than 0.2 times and less than 2 times. By controlling the mass ratio of the first component to the second component, the low temperature characteristics can be improved more significantly and well-balanced.

[0047] Examples of preferred compositions of the solvent of the liquid component include the following.

[0048] (i) A solvent in which 90% by mass or more of the glycol ether (G) is a dialkyl ether.

[0049] (ii) A solvent in which 90% by mass or more of the dialkyl ether in the glycol ether (G) is polyethylene glycol dialkyl ether.

[0050] (iii) A solvent in which 90% by mass or more of the dialkyl ether in the glycol ether (G) is polyethylene glycol dialkyl ether, and 90% by mole or more of the alkyl groups of the polyethylene glycol dialkyl ether are C1-C10 alkyl groups, C1-C5 alkyl groups, or C1-C3 alkyl groups.

[0051] (iv) 90% by mass or more of the glycol ether (G) is selected from ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, pentaethylene glycol monomethyl ether, hexaethylene glycol monomethyl ether, heptaethylene glycol monomethyl ether, octaethylene glycol monomethyl ether, nonaethylene glycol monomethyl ether, dodecaethylene glycol monomethyl ether, polyethylene glycol monomethyl ether 400, polyethylene glycol monomethyl ether 550, polyethylene glycol monomethyl ether 1000, polyethylene glycol monomethyl ether 2000, polyethylene glycol monomethyl ether 4000, a solvent of at least one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, polyethylene glycol dimethyl ether 240, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, ethylene glycol diethyl ether, diethylene glycol diethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol dibutyl ether, diethylene glycol dibutyl ether, ethylene glycol monohexyl ether and diethylene glycol monohexyl ether.

[0052] (v) 90 mass % or more of the glycol ether (G) is at least one solvent selected from polyethylene glycol monomethyl ether 400, polyethylene glycol monomethyl ether 550, polyethylene glycol monomethyl ether 1000, polyethylene glycol monomethyl ether 2000, polyethylene glycol monomethyl ether 4000, polyethylene glycol dimethyl ether 200, polyethylene glycol dimethyl ether 240, polyethylene glycol dimethyl ether 400, polyethylene glycol dimethyl ether 550, polyethylene glycol dimethyl ether 1000, polyethylene glycol dimethyl ether 2000, and polyethylene glycol dimethyl ether 4000.

[0053] Here, the numerical value of "Mn" in the expression of "polyethylene glycol monomethyl ether Mn" or "polyethylene glycol dimethyl ether Mn" represents an index of the number average molecular weight. Mn refers to a numerical range of Mn×0.8 or more and Mn×1.2 or less. For example, "polyethylene glycol dimethyl ether 400" refers to polyethylene glycol dimethyl ether having a number average molecular weight of 320 to 480.

[0054] In addition, Mn is the number average molecular weight calculated using gel permeation chromatography in terms of polystyrene.

[0055] The solute includes an acid component and an alkali component. As the solute, a salt of an acid component and an alkali component (electrolyte salt) can be used. The electrolyte salt dissociates at least partially in the liquid component to generate cations and anions. By making the solute include an acid component and an alkali component, the dissociation degree of the ions is improved, so the repairability of the dielectric layer can be improved. It should be noted that when preparing the liquid component, an electrolyte salt can be added to the solvent, an acid component and an alkali component can also be added, and an electrolyte salt, as well as an acid component and / or an alkali component can also be added.

[0056] As the acid component, an organic acid is preferred. As the organic acid, for example, an organic carboxylic acid or an anhydride thereof can be mentioned. As the organic acid, for example, an aromatic carboxylic acid, an aliphatic carboxylic acid, an alicyclic carboxylic acid, etc. can be mentioned. As the aromatic carboxylic acid, phthalic acid, isophthalic acid, terephthalic acid, benzoic acid, salicylic acid, trimellitic acid, pyromellitic acid, etc. can be mentioned. As the alicyclic carboxylic acid, maleic acid, adipic acid, etc. can be mentioned. As the alicyclic carboxylic acid, hydrides of aromatic carboxylic acids, etc. can be mentioned. From the viewpoint of high repairability and thermal stability of the dielectric layer, phthalic acid is preferred. The acid component can be used alone or in combination of two or more.

[0057] As the base component, an organic base is preferred. Examples of the organic base include amine compounds, quaternary amidine compounds, quaternary ammonium compounds, etc. The amine compound may be any of a primary amine, a secondary amine, and a tertiary amine. Examples of the amine compound include aliphatic amines, aromatic amines, heterocyclic amines, etc. The base component may be used alone or in combination of two or more.

[0058] Specific examples of the amine compound include methylamine, dimethylamine, monoethyldimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, N,N-diisopropylethylamine, tetramethylethylenediamine, hexamethylenediamine, spermidine, spermine, adamantane, aniline, phenethylamine, toluidine, pyrrolidine, piperidine, piperazine, morpholine, imidazole, imidazoline, pyridine, pyridazine, pyrimidine, pyrazine, and 4-dimethylaminopyridine.

[0059] As the quaternary amidinium compound, a quaternary compound of a cyclic amidine compound is preferred, and examples thereof include imidazolium compounds and imidazolinium compounds. As the quaternary imidazolium compound, examples thereof include 1,3-dimethylimidazolium, 1,2,3-trimethylimidazolium, 1-ethyl-3-methylimidazolium, 1-ethyl-2,3-dimethylimidazolium, 1,3-diethylimidazolium, 1,2-diethyl-3-methylimidazolium, and 1,3-diethyl-2-methylimidazolium. Examples of the quaternary imidazolinium compound include 1,3-dimethylimidazolinium, 1,2,3-trimethylimidazolinium, 1-ethyl-3-methylimidazolinium, 1-ethyl-2,3-dimethylimidazolinium, 1,3-diethylimidazolinium, 1,2-diethyl-3-methylimidazolinium, 1,3-diethyl-2-methylimidazolinium, and 1,2,3,4-tetramethylimidazolinium.

[0060] As the quaternary ammonium compound, for example, diethyldimethylammonium, monoethyltrimethylammonium, etc. are preferred.

[0061] From the viewpoint of suppressing degradation of the solid electrolyte and improving the repairability of the dielectric layer, the molar ratio of the acid component to the base component (=acid component / base component) is preferably 1.1 or more and 10.0 or less.

[0062] The concentration of the acid component in the liquid component is preferably 0.1% by mass or more and 30% by mass or less, more preferably 1% by mass or more and 20% by mass or less. The concentration of the alkali component in the liquid component is preferably 0.1% by mass or more and 20% by mass or less, more preferably 1% by mass or more and 15% by mass or less. In these cases, the repairability of the dielectric layer can be further improved.

[0063] Hereinafter, the present invention will be described in more detail based on the embodiments. However, the following embodiments do not limit the present invention.

[0064] Figure 1 is a schematic cross-sectional view of an electrolytic capacitor according to this embodiment, Figure 2 1 is a schematic diagram showing a portion of a capacitor element of the electrolytic capacitor being developed. Hereinafter, a cylindrical electrolytic capacitor will be described as an example, but the form of the electrolytic capacitor is not particularly limited.

[0065] The electrolytic capacitor includes, for example, a capacitor element 10, a cylindrical case 11 for accommodating the capacitor element 10, a sealing member 12 for blocking an opening of the case 11, a seat plate 13 for covering the sealing member 12, leads 14A and 14B extending from a through hole 12a of the sealing member 12 and penetrating the seat plate 13, and lead tabs 15A and 15B for connecting the leads 14A and 14B to electrodes of the capacitor element 10. The vicinity of the opening end of the case 11 is drawn inward, and the opening end is curled so as to be crimped to the sealing member 12.

[0066] The capacitor element 10 is composed of Figure 2 The wound body shown is produced. The wound body includes an anode body 21 connected to a lead tab 15A, a cathode body 22 connected to a lead tab 15B, and a separator 23. The wound body is a semi-finished product in which a solid electrolyte is not formed between the anode body 21 and the cathode body 22.

[0067] The anode body 21 and the cathode body 22 are wound with the separator 23 interposed therebetween. The outermost periphery of the wound body is fixed by a stopper band 24. It should be noted that Figure 2 This shows a partially unrolled state before the outermost circumference of the wound body is fixed.

[0068] The anode body 21 has a metal foil roughened in a manner that the surface has an uneven surface or the surface layer is porous. A dielectric layer is formed on the metal foil having an uneven surface or a porous portion. A solid electrolyte is attached to at least a portion of the surface of the dielectric layer. The solid electrolyte may cover at least a portion of the surface of the cathode body 22 and / or the surface of the diaphragm 23. The capacitor element 10 formed with the solid electrolyte is accommodated in the housing 11 together with the liquid component (not shown).

[0069] (Liquid ingredients)

[0070] The liquid component contains a solvent and a solute. The liquid component can be prepared by mixing the constituent components. The liquid component may be any of the liquid components described above.

[0071] (Capacitor Components)

[0072] Capacitor element 10 includes an anode body having a dielectric layer, a cathode body, and a solid electrolyte in contact with the dielectric layer. Capacitor element 10 generally includes a separator interposed between the anode body and the cathode body.

[0073] (Anode)

[0074] The anode body may be, for example, a metal foil with a roughened surface as described above. The type of metal constituting the metal foil is not particularly limited, but valve metals such as aluminum, tantalum, and niobium, and alloys containing valve metals are preferably used from the perspective of easily forming a dielectric layer.

[0075] The surface of the metal foil can be roughened by a known method. By roughening, a plurality of concave and convex surfaces are formed on the surface of the metal foil. The roughening is preferably performed by etching the metal foil, for example. The etching process can be performed by direct current electrolysis or alternating current electrolysis, for example.

[0076] (Dielectric layer)

[0077] The dielectric layer is formed on the surface of the anode body. Specifically, the dielectric layer is formed on the roughened surface of the metal foil, and is therefore formed along the inner wall surfaces of the holes and depressions (pits) on the surface of the anode body.

[0078] The method for forming the dielectric layer is not particularly limited, and the dielectric layer can be formed by subjecting the metal foil to a chemical conversion treatment. The chemical conversion treatment can be performed, for example, by immersing the metal foil in a chemical conversion treatment solution such as an ammonium adipate solution. In the chemical conversion treatment, a voltage can be applied as needed while the metal foil is immersed in the chemical conversion treatment solution.

[0079] Generally, from the viewpoint of mass productivity, a large piece of metal foil formed of a valve metal or the like is subjected to a roughening treatment and a chemical conversion treatment. In this case, the treated foil is cut into a desired size to prepare an anode body having a dielectric layer formed thereon.

[0080] (Cathode)

[0081] The cathode body may be made of, for example, metal foil. The type of metal is not particularly limited, but preferably a valve metal such as aluminum, tantalum, niobium, or an alloy containing a valve metal is used. The cathode body may be roughened and / or chemically converted as required. Roughening and chemical conversion may be performed, for example, by the methods described for the anode body.

[0082] (Diaphragm)

[0083] The separator is not particularly limited, and for example, nonwoven fabrics containing fibers of cellulose, polyethylene terephthalate, vinylon, or polyamide (for example, aliphatic polyamide, aromatic polyamide such as aramid) can be used.

[0084] (Solid Electrolyte)

[0085] The solid electrolyte includes, for example, a conductive polymer. As the conductive polymer, for example, a π-conjugated polymer can be used. The conductive polymer may include a π-conjugated polymer and a dopant.

[0086] As π-conjugated polymers, for example, polypyrrole, polythiophene, polyfuran, polyaniline, and their derivatives can be used. Derivatives refer to polymers with polypyrrole, polythiophene, polyfuran, polyaniline, etc. as basic skeletons. For example, polythiophene derivatives include poly(3,4-ethylenedioxythiophene) (PEDOT) and the like.

[0087] As the dopant, a polymer such as polystyrenesulfonic acid (PSS) can be used, or naphthalenesulfonic acid, toluenesulfonic acid, or the like can be used.

[0088] The conductive polymer can be formed, for example, by chemically polymerizing and / or electrolytically polymerizing the precursor of the conjugated polymer (monomer, oligomer, etc.) on the dielectric layer. In this case, the precursor of the conjugated polymer can coexist with the dopant. A solution in which the conductive polymer (and the dopant) is dissolved or a dispersion in which the conductive polymer (and the dopant) is dispersed can also be applied to the dielectric layer and dried to form a solid electrolyte.

[0089] (other)

[0090] The capacitor element 10 can be manufactured by a known method. For example, the capacitor element 10 can be manufactured by stacking an anode body and a cathode body with a dielectric layer formed thereon with a separator interposed therebetween, and then forming a solid electrolyte layer between the anode body and the cathode body. Alternatively, the capacitor element 10 can be manufactured by winding an anode body and a cathode body with a dielectric layer formed thereon with a separator interposed therebetween. Figure 2 The wound body shown in FIG. 1 is produced by forming a solid electrolyte layer between the anode body and the cathode body. When forming the wound body, the lead tabs 15A and 15B are wound while being wound, so that Figure 2 As shown, the leads 14A and 14B can be grown from the wound body.

[0091] Among the anode body, cathode body and separator, the outermost component of the wound body (in Figure 2 The end of the outer surface of the cathode body 22 is fixed with a stop tape. It should be noted that when the anode body is prepared by cutting a large piece of metal foil, in order to provide a dielectric layer on the cut surface of the anode body, the capacitor element in the state of the winding body can be further subjected to chemical conversion treatment.

[0092] The electrolytic capacitor can be manufactured by housing capacitor element 10 and the prepared liquid component in case 11 and sealing the opening of case 11 with sealing member 12 .

[0093] [Example]

[0094] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0095] 《Examples 1 to 8》

[0096] In this example, a wound electrolytic capacitor (diameter 10 mm×length 10 mm) having a rated voltage of 63 V and a rated capacitance of 82 μF was produced. A specific method for producing the electrolytic capacitor will be described below.

[0097] (Fabrication of capacitor elements)

[0098] The Al foil (anode body) whose surface has been roughened is subjected to chemical conversion treatment using ammonium adipate solution to form a dielectric layer. The obtained anode foil is cut into a specified size. Lead connectors are connected to the Al foils serving as the anode foil and the cathode foil, respectively, and the anode foil and the cathode foil are wound across the diaphragm, and the outer surface is fixed with a stop tape to thereby produce a wound body. At this time, the lead connector and the lead integrated with the lead connector are wound while being drawn out from the wound body. The wound body is further subjected to chemical conversion treatment again using an ammonium adipate solution.

[0099] The wound body is immersed in a dispersion containing polyethylene dioxythiophene (conductive polymer), polystyrene sulfonic acid (dopant) and water stored in a specified container for 5 minutes, and then the wound body is lifted from the dispersion. Next, the wound body impregnated with the dispersion is dried in a drying oven at 150°C for 20 minutes to allow the conductive polymer and the dopant to adhere between the anode foil and the cathode foil of the wound body. In this way, the capacitor element is completed and stored in a bottomed cylindrical case with a diameter of 10 mm and a length of 10 mm.

[0100] (Liquid component impregnation)

[0101] The liquid component is injected into the shell, and the liquid component is impregnated into the capacitor element in a reduced pressure atmosphere (40 kPa). As the liquid component, a solution of triethylamine phthalate as a solute (electrolyte salt) dissolved in a solvent of the composition shown in Table 1 is used. In the liquid component, the concentration of the electrolyte salt is uniformly 13 mass % (the total of the solute (electrolyte salt) + solvent = 100%).

[0102] (Sealing of capacitor elements)

[0103] The capacitor element impregnated with the liquid component is sealed to complete the electrolytic capacitor. Specifically, the capacitor element is housed in a bottomed shell so that the lead wire is located on the open side of the bottomed shell, and a sealing member (an elastic material containing butyl rubber as a rubber component) formed in a way that the lead wire passes through is arranged above the capacitor element, and the capacitor element is sealed in the bottomed shell. Then, a deep drawing process is performed near the open end of the bottomed shell, and the open end is further curled, and a seat plate is arranged on the curled portion, thereby completing the process. Figure 1 The electrolytic capacitor shown in the figure is then aged while voltage is applied.

[0104] Comparative Example 1

[0105] A liquid component was prepared in the same manner as in Example 1, and an electrolytic capacitor was assembled, except that polyethylene glycol (Mn: 200) was used instead of the glycol ether.

[0106] Comparative Example 2

[0107] A liquid component was prepared in the same manner as in Example 1, and an electrolytic capacitor was assembled, except that polyethylene glycol (Mn: 400) was used instead of the glycol ether.

[0108] [evaluate]

[0109] Using the electrolytic capacitors obtained in the examples and comparative examples, the electrostatic capacitance, tanδ, and ESR at 20°C and -55°C were measured at 120 Hz according to the following steps, and the rate of change when the value at 20°C was set to 100% was calculated. The results are shown in Table 2. Examples 1 to 8 are A1 to A8, respectively, and Comparative Examples 1 to 2 are B1 to B2, respectively. In the test, 10 electrolytic capacitors randomly selected from 100 produced in each example were measured, and the average value was calculated.

[0110] [Table 1]

[0111]

[0112] The meanings of the abbreviations in Table 1 and Table 2 are as follows.

[0113] EG: Ethylene glycol

[0114] SL: Sulfolane

[0115] PEG: polyethylene glycol

[0116] MME: Monomethyl ether

[0117] DME: dimethyl ether

[0118] The values ​​after PEG, MME and DME (200, 300, 400) are the number average molecular weights.

[0119] Cap.: electrostatic capacitance

[0120] [Table 2]

[0121]

[0122] As shown in Tables 1 and 2, even at room temperature (20°C), in Examples A1 to A8, a tendency of slightly increasing electrostatic capacitance was observed compared with Comparative Examples B1 to B2, and a tendency of slightly decreasing tanδ and ESR was observed. However, the superiority of the examples at room temperature is extremely small. On the other hand, at minus 55°C, in Examples A1 to A8, a tendency of significantly increasing electrostatic capacitance was observed compared with Comparative Examples B1 to B2, and a tendency of significantly decreasing tanδ and ESR was observed. Among them, when dialkyl ether was used, the electrostatic capacitance at low temperature increased significantly. In addition, by using not only the first component but also the second component in combination, a further improvement in electrostatic capacitance was observed. Among them, when dialkyl ether was used as the first component and the second component was used in combination, the result was a good balance of low temperature characteristics.

[0123] Industrial Applicability

[0124] The electrolytic capacitor of the present invention has a high capacity even at low temperatures (eg, temperatures of -50°C or less) and is excellent in low-temperature characteristics, and can therefore be used in various applications.

[0125] The preferred embodiments of the present invention are described, but such disclosure should not be interpreted in a limiting manner. By reading the above disclosure, various deformations and changes are obvious to those skilled in the art belonging to the technical field of the present invention. Therefore, the scope of the attached claims should be interpreted as including all deformations and changes without departing from the true spirit and scope of the present invention.

[0126] Description of Reference Numerals

[0127] 10: capacitor element, 11: housing, 12: sealing member, 13: seat plate, 14A, 14B: lead wires, 15A, 15B: lead wire connectors, 21: anode body, 22: cathode body, 23: diaphragm, 24: anti-rolling tape

Claims

1. An electrolytic capacitor comprising a capacitor element and a liquid component, The capacitor element includes an anode body having a dielectric layer and a solid electrolyte in contact with the dielectric layer. The liquid component comprises a solvent and a solute, The solvent contains a glycol ether as a first component, The glycol ether comprises at least one selected from monoalkyl ether and dialkyl ether, The glycol ether has -(CH2O) n -structure, n is an integer of 1 or more.

2. The electrolytic capacitor according to claim 1, wherein: The content of the glycol ether in the liquid component is 10% by mass or more.

3. The electrolytic capacitor according to claim 1, wherein: 90% by mass or more of the glycol ethers have an integer n within a range of 1 to 11.

4. The electrolytic capacitor according to claim 1, wherein: The number average molecular weight of the glycol ether is 100 or more and 1000 or less.

5. The electrolytic capacitor according to claim 1, wherein: The content of the dialkyl ether in the glycol ether exceeds 50% by mass.

6. The electrolytic capacitor according to any one of claims 1 to 5, wherein 90 mol% or more of the alkyl groups contained in the glycol ether are C1-C10 alkyl groups having 1 to 10 carbon atoms.

7. The electrolytic capacitor according to claim 6, wherein: 90 mol % or more of the alkyl groups of the monoalkyl ether are C1-C10 alkyl groups.

8. The electrolytic capacitor according to claim 6, wherein: 90 mol% or more of the alkyl groups of the dialkyl ether are independently C1-C10 alkyl groups.

9. The electrolytic capacitor according to any one of claims 1 to 5, wherein The content of the glycol ether in the liquid component is 70% by mass or less.

10. The electrolytic capacitor according to any one of claims 1 to 5, wherein The solvent further contains at least one selected from ethylene glycol and sulfolane as a second component.

11. The electrolytic capacitor according to claim 10, wherein: The solvent further contains γ-butyrolactone as a third component.

12. The electrolytic capacitor according to claim 10, wherein: The mass of the first component is not less than 0.1 times and not more than 5 times the mass of the second component.

13. The electrolytic capacitor according to any one of claims 1 to 5, wherein: The solute contains an acid component and a base component.

14. The electrolytic capacitor according to any one of claims 1 to 5, wherein: 90% by mass or more of the dialkyl ether is polyethylene glycol dialkyl ether, 90 mol % or more of the alkyl groups in the polyethylene glycol dialkyl ether are C1-C10 alkyl groups having 1 to 10 carbon atoms.

15. The electrolytic capacitor according to any one of claims 1 to 5, wherein More than 90% by mass of the glycol ether is selected from ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, pentaethylene glycol monomethyl ether, hexaethylene glycol monomethyl ether, heptaethylene glycol monomethyl ether, octaethylene glycol monomethyl ether, nonaethylene glycol monomethyl ether, dodecaethylene glycol monomethyl ether, polyethylene glycol monomethyl ether 400, polyethylene glycol monomethyl ether 550, polyethylene glycol monomethyl ether 1000, polyethylene glycol monomethyl ether 2000, polyethylene glycol monomethyl ether 4000, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether , polyethylene glycol dimethyl ether 200, polyethylene glycol dimethyl ether 240, polyethylene glycol dimethyl ether 400, polyethylene glycol dimethyl ether 550, polyethylene glycol dimethyl ether 1000, polyethylene glycol dimethyl ether 2000, polyethylene glycol dimethyl ether 4000, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, ethylene glycol diethyl ether, diethylene glycol diethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol dibutyl ether, diethylene glycol dibutyl ether, ethylene glycol monohexyl ether and diethylene glycol monohexyl ether.