Rapid permeation 3D core body and preparation method thereof
By using modified wood pulp fiber layer and tackified modified polyurethane hot melt adhesive in the diaper core, the problem of easy destruction of wood pulp fiber layer when absorbing urine is solved, achieving more stable urine distribution and better wear comfort.
Patent Information
- Application Number
- CN202411088914.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
AI Technical Summary
The wood pulp fiber layer in the core of traditional diapers is easily damaged when absorbing urine, resulting in uneven distribution of urine, affecting the shape of the core and wearing comfort.
Using a modified wood pulp fiber layer, the structural stability of the modified wood pulp fiber layer is improved by mixing 3-5 wt% low-melting fiber into the wood pulp fiber, and using tackified modified polyurethane hot melt adhesive as the bonding layer. , prevent it from gathering towards the middle of the core.
It improves the structural stability and rapid permeability of the core, prevents changes in the core form caused by urine concentration, and improves wearable comfort and leak-proof performance.
Smart Images

Figure CN118975890A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of core materials, and in particular to a fast-penetrating 3D core and a preparation method thereof. Background Art
[0002] The core of the diaper is the key part for absorbing urine, and usually includes a surface layer, a first connecting layer, a polymer absorption layer, a second connecting layer and a bottom film layer. In order to improve the rapid penetration performance of the core, a wood pulp fiber layer can be added between the surface layer and the polymer absorption layer.
[0003] However, since the traditional wood pulp fiber layer is made of wood pulp fibers, when the core absorbs a large amount of urine, the structure of the wood pulp fiber layer is easily damaged and tends to gather in the middle of the core, affecting the uniform distribution of urine in the diaper, causing the shape of the diaper core to change, affecting the wearing comfort. Summary of the invention
[0004] In order to improve the problem in the related art that the structure of the wood pulp fiber layer is easily damaged and easily gathers in the middle of the core, the present application provides a fast-penetrating 3D core and a preparation method thereof.
[0005] In the first aspect, the present application provides a fast penetration 3D core adopting the following technical solution: A fast-penetrating 3D core comprises a surface layer, a first adhesive layer, a modified wood pulp fiber layer, a second adhesive layer, a polymer absorption layer, a third adhesive layer and a bottom film layer which are arranged in sequence from top to bottom, wherein the modified wood pulp fiber layer is obtained by uniformly mixing, molding and drying 3-5wt% low-melting-point fibers and 95-97wt% wood pulp fibers in sequence, and the two ends of the bottom film layer are folded toward the middle and fixed on the side of the surface layer away from the first adhesive layer.
[0006] The present application adopts a modified wood pulp fiber layer to replace the traditional wood pulp fiber layer, wherein the modified wood pulp fiber layer is mixed with 3-5wt% low melting point fiber (low melting point fiber generally refers to the fiber whose cortex can melt and produce bonding effect after heating to 110-150°C). After the low melting point fiber melts, it can improve the bonding strength between wood pulp fibers, improve the structural stability of the modified wood pulp fiber layer, and reduce the possibility that the modified wood pulp fiber layer is easily damaged and gathers in the middle of the core. It should be noted that the amount of low melting point fiber added should not be too large, otherwise it will easily affect the rapid diffusion and permeability of urine.
[0007] In some specific embodiments, the low-melting point fiber has a length of 0.1-0.2 mm, and the wood pulp fiber has a length of 0.5-1 mm.
[0008] In the present application, the low-melting point fibers within the above-mentioned length range are mixed with the wood pulp fibers, which is beneficial to the uniform dispersion of the low-melting point fibers in the wood pulp fibers and is beneficial to further improving the structural stability of the modified wood pulp fiber layer.
[0009] In some specific embodiments, the low melting point fiber is a hydroxyl-terminated saturated polyester resin fiber, and the first adhesive layer, the second adhesive layer, and the third adhesive layer are all made of a tackified modified polyurethane hot melt adhesive; The tackified modified polyurethane hot melt adhesive comprises 25.6-30.4 parts by weight of polyester diol, 15.8-20.5 parts by weight of isocyanate, 0.01-0.015 parts by weight of catalyst, 1.4-1.8 parts by weight of chain extender, 5.5-6.8 parts by weight of epoxy resin and 1.5-2.5 parts by weight of rosin pentaerythritol ester.
[0010] In the present application, the low-melting point fiber adopts end-hydroxyl saturated polyester resin fiber, and the first bonding layer, the second bonding layer, and the third bonding layer all adopt thickening modified polyurethane hot melt adhesive. Under the joint action of the first bonding layer and the second bonding layer, the structure of the modified wood pulp fiber layer can be further stabilized to prevent the problem of the modified wood pulp fiber layer gathering towards the middle of the core.
[0011] In some specific embodiments, the molecular weight of the polyester diol is 1000-3000, and more preferably 2000-3000.
[0012] In the present application, controlling the molecular weight of the polyester diol is beneficial to obtaining a tackified modified polyurethane hot melt adhesive with strong bonding ability.
[0013] In some specific embodiments, the epoxy resin is at least one of epoxy resin E44 and epoxy resin E51.
[0014] In some specific embodiments, the isocyanate is at least one of 1,4-cyclohexane diisocyanate, isophorone diisocyanate, and 4,4'-diphenylmethane diisocyanate.
[0015] In some specific embodiments, the chain extender is at least one of ethylene glycol, propylene glycol, 1,4-butanediol, and pentanediol.
[0016] In some specific embodiments, the preparation method of the tackified modified polyurethane hot melt adhesive comprises the following steps: heating the polyester diol to 50-55° C., then adding isocyanate and a catalyst, heating to 60-70° C., reacting for 1-1.5 hours, then adding a chain extender, and continuing the reaction for 0.5-1 hour to obtain a polyurethane hot melt adhesive; Epoxy resin and rosin pentaerythritol ester are added to the polyurethane hot melt adhesive, heated to 100-105° C., melted evenly, granulated, and cooled to obtain a tackified modified polyurethane hot melt adhesive.
[0017] In the present application, a polyurethane hot melt adhesive is first prepared using polyester diol, isocyanate and a chain extender, and then the polyurethane hot melt adhesive is tackified and modified with epoxy resin and rosin pentaerythritol ester, which is beneficial to the uniform dispersion of epoxy resin and rosin pentaerythritol ester in the polyurethane hot melt adhesive, thereby obtaining a tackified modified polyurethane hot melt adhesive with strong bonding force and the ability to effectively improve the structural stability of the modified wood pulp fiber layer.
[0018] In some specific embodiments, the drying temperature of the modified wood pulp fiber layer is 130-140°C.
[0019] The drying temperature of the modified wood pulp fiber layer is controlled at 130-140° C., which is beneficial to further improve the structural stability of the modified wood pulp fiber layer.
[0020] In the second aspect, the present application provides a method for preparing a fast-penetrating 3D core using the following technical solution: A method for preparing a fast-penetrating 3D core comprises the following steps: forming the first adhesive layer on one surface of the surface layer; Compounding the modified wood pulp fiber layer on the side of the first adhesive layer away from the surface layer; forming the second bonding layer on the side of the modified wood pulp fiber layer away from the first bonding layer; Spreading polymer water-absorbing particles on the second adhesive layer to form the polymer absorption layer; forming the third adhesive layer on one surface of the base film layer; Compounding the third adhesive layer with the polymer absorption layer; The two ends of the bottom film layer are folded toward the middle and bonded to the side of the surface layer away from the first bonding layer, and then edge-sealed and divided to obtain a fast-penetrating 3D core.
[0021] The 3D core prepared by the above method in the present application has both rapid permeability and structural stability, and has good leak-proof performance.
[0022] In summary, this application at least includes the following beneficial technical effects: (1) The present application adopts a modified wood pulp fiber layer to replace the traditional wood pulp fiber layer, wherein the modified wood pulp fiber layer is mixed with 3-5wt% low melting point fiber, which can improve the bonding strength between wood pulp fibers after melting, improve the structural stability of the modified wood pulp fiber layer, and reduce the possibility that the modified wood pulp fiber layer is easily damaged and gathers in the middle of the core. It should be noted that the amount of low melting point fiber added should not be too large, otherwise it will easily affect the rapid diffusion and permeability of urine.
[0023] (2) In the present application, the low melting point fiber adopts end-hydroxyl saturated polyester resin fiber, and the first bonding layer, the second bonding layer, and the third bonding layer all adopt thickening modified polyurethane hot melt adhesive. Under the joint action of the first bonding layer and the second bonding layer, the structure of the modified wood pulp fiber layer can be further stabilized, and the problem of the modified wood pulp fiber layer gathering toward the middle of the core can be prevented. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the structure of the fast-penetrating 3D core of the present application.
[0025] Description of reference numerals: 1. Surface layer; 2. First bonding layer; 3. Modified wood pulp fiber layer; 4. Second bonding layer; 5. Polymer absorption layer; 6. Third bonding layer; 7. Bottom film layer. DETAILED DESCRIPTION
[0026] The present application is further described below in conjunction with specific experiments. Example
[0027] [Example 1] A fast-penetrating 3D core comprises a surface layer 1, a first adhesive layer 2, a modified wood pulp fiber layer 3, a second adhesive layer 4, a polymer absorption layer 5, a third adhesive layer 6 and a bottom film layer 7, which are arranged in sequence from top to bottom. Among them, the surface layer 1 is made of dust-free paper, the bottom film layer 7 is made of hot air cloth, and the two ends of the bottom film layer 7 are folded toward the middle and fixed on the side of the surface layer 1 away from the first adhesive layer 2. The modified wood pulp fiber layer 3 is obtained by uniformly mixing and molding 3wt% low-melting point fiber and 97wt% wood pulp fiber in turn, and then drying at 130-140°C. In this embodiment, the low-melting point fiber specifically adopts ES fiber, and the length of the ES fiber is 0.1-0.2mm, the melting point is 125-135°C, and the length of the wood pulp fiber is 0.5-1mm; the first adhesive layer 2, the second adhesive layer 4, and the third adhesive layer 6 all adopt polyurethane hot melt adhesive.
[0028] The polyurethane hot melt adhesive comprises 25.6 kg of polycaprolactone diol with a molecular weight of 2000, 15.8 kg of 4,4'-diphenylmethane diisocyanate, 0.01 kg of dibutyltin dilaurate and 5.4 kg of propylene glycol. The preparation method of the polyurethane hot melt adhesive comprises the following steps: The polycaprolactone diol was heated to 50°C, and then 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate were added, the temperature was raised to 60°C, the reaction was continued for 1.5 hours, and then propylene glycol was added, the reaction was continued for 1 hour, and then granulation and cooling were performed to obtain a polyurethane hot melt adhesive.
[0029] In this embodiment, the preparation method of the fast permeable 3D core comprises the following steps: Forming a first adhesive layer 2 on one surface of the surface layer 1; Compounding the modified wood pulp fiber layer 3 on the side of the first adhesive layer 2 facing away from the surface layer 1; A second adhesive layer 4 is formed on the side of the modified wood pulp fiber layer 3 facing away from the first adhesive layer 2; Spreading polymer water-absorbing particles on the second adhesive layer 4 to form a polymer absorption layer 5; Forming a third adhesive layer 6 on one surface of the base film layer 7; Compounding the third adhesive layer 6 with the polymer absorption layer 5; The two ends of the bottom film layer 7 are folded toward the middle and bonded to the side of the surface layer 1 away from the first bonding layer 2, and then sealed and divided to obtain a fast-penetrating 3D core.
[0030] [Example 2] A fast-penetrating 3D core comprises a surface layer 1, a first adhesive layer 2, a modified wood pulp fiber layer 3, a second adhesive layer 4, a polymer absorption layer 5, a third adhesive layer 6 and a bottom film layer 7, which are arranged in sequence from top to bottom. Among them, the surface layer 1 is made of dust-free paper, the bottom film layer 7 is made of hot air cloth, and the two ends of the bottom film layer 7 are folded toward the middle and fixed on the side of the surface layer 1 away from the first adhesive layer 2. The modified wood pulp fiber layer 3 is obtained by uniformly mixing and molding 5wt% low-melting point fiber and 95wt% wood pulp fiber in turn, and then drying at 130-140°C. In this embodiment, the low-melting point fiber is specifically ES fiber, and the length of the low-melting point fiber is 0.1-0.2mm, the melting point is 125-135°C, and the length of the wood pulp fiber is 0.5-1mm; the first adhesive layer 2, the second adhesive layer 4, and the third adhesive layer 6 are all made of polyurethane hot melt adhesive.
[0031] The polyurethane hot melt adhesive comprises 25.6 kg of polycaprolactone diol with a molecular weight of 2000, 15.8 kg of 4,4'-diphenylmethane diisocyanate, 0.01 kg of dibutyltin dilaurate and 5.4 kg of propylene glycol. The preparation method of the polyurethane hot melt adhesive comprises the following steps: The polycaprolactone diol was heated to 50°C, and then 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate were added, the temperature was raised to 60°C, the reaction was continued for 1.5 hours, and then propylene glycol was added, the reaction was continued for 1 hour, and then granulation and cooling were performed to obtain a polyurethane hot melt adhesive.
[0032] In this embodiment, the preparation method of the fast permeable 3D core comprises the following steps: Forming a first adhesive layer 2 on one surface of the surface layer 1; Compounding the modified wood pulp fiber layer 3 on the side of the first adhesive layer 2 facing away from the surface layer 1; A second adhesive layer 4 is formed on the side of the modified wood pulp fiber layer 3 facing away from the first adhesive layer 2; Spreading polymer water-absorbing particles on the second adhesive layer 4 to form a polymer absorption layer 5; Forming a third adhesive layer 6 on one surface of the base film layer 7; Compounding the third adhesive layer 6 with the polymer absorption layer 5; The two ends of the bottom film layer 7 are folded toward the middle and bonded to the side of the surface layer 1 away from the first bonding layer 2, and then sealed and divided to obtain a fast-penetrating 3D core.
[0033] [Example 3] A fast-penetrating 3D core, which differs from [Example 1] in that: In this embodiment, the low melting point fiber is specifically a hydroxyl-terminated saturated polyester resin fiber, the hydroxyl-terminated saturated polyester resin fiber has a length of 0.1-0.2 mm and a softening point of 102-112°C.
[0034] [Example 4] A fast-penetrating 3D core, which differs from [Example 1] in that: In this embodiment, the first adhesive layer 2, the second adhesive layer 4, and the third adhesive layer 6 all use a tackified modified polyurethane hot melt adhesive. In this embodiment, the tackified modified polyurethane hot melt adhesive includes 25.6 kg of polycaprolactone diol with a molecular weight of 2000, 15.8 kg of 4,4'-diphenylmethane diisocyanate, 0.01 kg of dibutyltin dilaurate, 1.4 kg of propylene glycol, 5.5 kg of epoxy resin E44, and 1.5 kg of 145 rosin pentaerythritol ester. The preparation method of the tackified modified polyurethane hot melt adhesive includes the following steps: heating the polycaprolactone diol to 50° C., then adding 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate, heating to 60° C., reacting for 1.5 hours, then adding propylene glycol, and continuing to react for 1 hour to obtain a polyurethane hot melt adhesive; Epoxy resin and 145 rosin pentaerythritol ester are added to the polyurethane hot melt adhesive, heated to 100°C, melted evenly, granulated, and cooled to obtain a tackified modified polyurethane hot melt adhesive.
[0035] [Example 5] A fast-penetrating 3D core, which differs from [Example 1] in that: In this embodiment, the low melting point fiber specifically adopts hydroxyl-terminated saturated polyester resin fiber, the length of hydroxyl-terminated saturated polyester resin fiber is 0.1-0.2mm, and the softening point is 102-112°C. The first adhesive layer 2, the second adhesive layer 4, and the third adhesive layer 6 all adopt tackified modified polyurethane hot melt adhesive. In this embodiment, the tackified modified polyurethane hot melt adhesive includes 25.6kg of polycaprolactone diol with a molecular weight of 2000, 15.8kg4,4'-diphenylmethane diisocyanate, 0.01kg dibutyltin dilaurate, 1.4kg propylene glycol, 5.5kg epoxy resin E44 and 1.5kg145 rosin pentaerythritol ester. The preparation method of the tackified modified polyurethane hot melt adhesive includes the following steps: The polycaprolactone diol was heated to 50°C, and then 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate were added, and the temperature was raised to 60°C, and the reaction was carried out for 1.5 hours, and then propylene glycol was added, and the reaction was continued for 1 hour to obtain a polyurethane hot melt adhesive; Epoxy resin and 145 rosin pentaerythritol ester are added to the polyurethane hot melt adhesive, heated to 100°C, melted evenly, granulated, and cooled to obtain a tackified modified polyurethane hot melt adhesive.
[0036] [Example 6] A fast-penetrating 3D core, which differs from [Example 5] in that: The tackified modified polyurethane hot melt adhesive includes 30.4 kg of polycaprolactone diol with a molecular weight of 2000, 20.5 kg of 4,4'-diphenylmethane diisocyanate, 0.015 kg of dibutyltin dilaurate, 1.8 kg of propylene glycol, 6.8 kg of epoxy resin E44 and 2.5 kg of 145 rosin pentaerythritol ester. The preparation method of the tackified modified polyurethane hot melt adhesive includes the following steps: The polycaprolactone diol was heated to 55°C, and then 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate were added, and the temperature was raised to 70°C, and the reaction was continued for 1 hour, and then propylene glycol was added, and the reaction was continued for 1 hour to obtain a polyurethane hot melt adhesive; Epoxy resin and 145 rosin pentaerythritol ester are added to the polyurethane hot melt adhesive, heated to 105°C, melted evenly, granulated, and cooled to obtain a tackified modified polyurethane hot melt adhesive.
[0037] [Example 7] A fast-penetrating 3D core, which differs from [Example 5] in that: the amount of 4,4'-diphenylmethane diisocyanate used is 10 kg.
[0038] [Example 8] A fast-penetrating 3D core, which differs from [Example 5] in that the epoxy resin E44 is replaced by an equal amount of 145 rosin pentaerythritol ester.
[0039] [Example 9] A fast-penetrating 3D core, which differs from [Example 5] in that 145 rosin pentaerythritol ester is replaced by an equal amount of epoxy resin E44.
[0040] Comparative Example [Comparative Example 1] A 3D core, which differs from [Example 1] in that: In the modified wood pulp fiber layer 3, the weight proportion of the low melting point fiber is 10 wt%, and the weight proportion of the wood pulp fiber is 90 wt%.
[0041] [Comparative Example 2] A 3D core, which differs from [Example 1] in that: The low melting point fibers are replaced by an equal amount of wood pulp fibers, that is, the modified wood pulp fiber layer 3 is replaced by a common wood pulp fiber layer.
[0042] Performance testing (1) Core absorption performance test: The absorption rate and rewet amount of the core sample were tested with reference to QB / T 5650-2021 "Composite absorbent core for disposable paper sanitary products". The test results are recorded in Table 1.
[0043] (2) Core stability test: The cores of the embodiments and comparative examples were solidified at both ends and the bottom of the cores were ensured to be unsupported. 1000 g and 1500 g of 0.9% saline were added to the middle of the cores of the embodiments and comparative examples, respectively. The state of the cores after water absorption was recorded in Table 2.
[0044] Table 1 Sample Absorption rate / s Re-seepage amount / g Example 1 5-10 0.39 Example 2 5-10 0.33 Example 3 5-10 0.36 Example 4 5-10 0.35 Example 5 5-10 0.38 Example 6 5-10 0.34 Example 7 5-10 0.36 Example 8 5-10 0.33 Example 9 5-10 0.34 Comparative Example 1 20-25 0.67 Comparative Example 2 5-10 0.36 Table 2 Combining Example 1 with Comparative Example 1 and the data in Tables 1-2, it can be seen that the amount of low-melting-point fiber added to the modified wood pulp fiber layer should not be too large, as it will easily affect the rapid permeability of the core.
[0045] Combining Example 1 with Comparative Example 2 and the data in Tables 1-2, it can be seen that when a traditional wood pulp fiber layer is used instead of the modified wood pulp fiber layer of the present application, when the core absorbs a lot of liquid, the structure of the wood pulp fiber layer is destroyed, resulting in uneven liquid diversion, and the liquid is concentrated in the middle, and the middle of the core is prone to clumping.
[0046] Combining Example 1 with Examples 3-5 and the data in Table 1-2, it can be seen that when the low-melting point fiber in the modified wood pulp fiber layer is made of end-hydroxyl saturated polyester resin fiber, and the first bonding layer, the second bonding layer and the third bonding layer are respectively made of epoxy resin and rosin pentaerythritol ester to obtain a thickened modified polyurethane hot melt adhesive, it is beneficial to further improve the structural stability of the modified wood pulp fiber layer in the core body, promote uniform flow of the liquid, and make it less likely for lumps to appear in the middle of the core body.
[0047] Combining Example 5 with Examples 7-9 and the data in Table 1-2, it can be seen that the amount of each component in the tackified modified polyurethane hot melt adhesive, epoxy resin and rosin pentaerythritol ester all play a key role in further improving the stability of the modified wood pulp fiber layer in the core, and none of them can be missing.
[0048] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A fast-penetrating 3D core, Features: The invention comprises a surface layer (1), a first adhesive layer (2), a modified wood pulp fiber layer (3), a second adhesive layer (4), a polymer absorption layer (5), a third adhesive layer (6) and a bottom film layer (7) which are arranged in sequence from top to bottom, wherein the modified wood pulp fiber layer (3) is obtained by uniformly mixing, molding and drying 3-5wt% of low melting point fibers and 95-97wt% of wood pulp fibers in sequence, and the two ends of the bottom film layer (7) are folded toward the middle and fixed on the side of the surface layer (1) away from the first adhesive layer (2).
2. A fast permeable 3D core according to claim 1, Features: The length of the low-melting-point fiber is 0.1-0.2 mm, and the length of the wood pulp fiber is 0.5-1 mm.
3. A fast permeable 3D core according to claim 2, Features: The low melting point fiber is a hydroxyl-terminated saturated polyester resin fiber, and the first adhesive layer (2), the second adhesive layer (4), and the third adhesive layer (6) are all made of a tackified modified polyurethane hot melt adhesive; The tackified modified polyurethane hot melt adhesive comprises 25.6-30.4 parts by weight of polyester diol, 15.8-20.5 parts by weight of isocyanate, 0.01-0.015 parts by weight of catalyst, 1.4-1.8 parts by weight of chain extender, 5.5-6.8 parts by weight of epoxy resin and 1.5-2.5 parts by weight of rosin pentaerythritol ester.
4. A fast permeable 3D core according to claim 3, Features: The molecular weight of the polyester diol is 2000-3000.
5. A fast permeable 3D core according to claim 3, Features: The epoxy resin is at least one of epoxy resin E44 and epoxy resin E51.
6. A fast permeable 3D core according to claim 3, Features: The isocyanate is at least one of 1,4-cyclohexane diisocyanate, isophorone diisocyanate and 4,4'-diphenylmethane diisocyanate.
7. A fast permeable 3D core according to claim 3, Features: The chain extender is at least one of ethylene glycol, propylene glycol, 1,4-butanediol and pentanediol.
8. A fast permeable 3D core according to any one of claims 3 to 7, Features: The preparation method of the tackified modified polyurethane hot melt adhesive comprises the following steps: Heat the polyester diol to 50-55°C, then add isocyanate and catalyst, raise the temperature to 60-70°C, react for 1-1.5h, then add chain extender, continue to react for 0.5-1h, and obtain polyurethane hot melt adhesive; Epoxy resin and rosin pentaerythritol ester are added to the polyurethane hot melt adhesive, heated to 100-105° C., melted evenly, granulated, and cooled to obtain a tackified modified polyurethane hot melt adhesive.
9. A fast permeable 3D core according to any one of claims 1 to 7, Features: The drying temperature of the modified wood pulp fiber layer (3) is 130-140°C.
10. A method for preparing a fast permeable 3D core according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Forming the first adhesive layer (2) on one surface of the surface layer (1); Compounding the modified wood pulp fiber layer (3) on the side of the first adhesive layer (2) facing away from the surface layer (1); Forming the second adhesive layer (4) on the side of the modified wood pulp fiber layer (3) facing away from the first adhesive layer (2); Spreading polymer water-absorbing particles on the second adhesive layer (4) to form the polymer absorption layer (5); Forming the third adhesive layer (6) on one surface of the base film layer (7); Compounding the third adhesive layer (6) and the polymer absorption layer (5); The two ends of the bottom film layer (7) are folded toward the middle and bonded to the side of the surface layer (1) away from the first bonding layer (2), and then edge-sealed and divided to obtain a fast-penetrating 3D core.