Metal ion polyphenol coating material as well as preparation method and application thereof
By forming a metal ion polyphenol coating on the substrate, using the combination of strontium ions and Cu2+/Zn2+, the problem of insufficient inhibition of endothelial cell proliferation and smooth muscle cell in existing materials is solved, and better biological activity and heart Vascular protection effect.
Patent Information
- Application Number
- CN202411101920.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-19
AI Technical Summary
The existing materials deposited on substrates using metal polyphenol networks (MPNs) are insufficient in promoting endothelial cell adhesion and proliferation ability and inhibiting smooth muscle cell adhesion and proliferation ability.
The metal ion polyphenol coating material is used, and the coordination and cation π-interaction method are combined by the combination of strontium ions and copper ions or zinc ions, and a uniform polyphenol coating is formed to improve the biological activity of the material.
It significantly improves the ability of the material to promote the adhesion and proliferation of endothelial cells, while inhibiting the adhesion and proliferation of smooth muscle cells, enhances the anti-inflammatory and myocardial repair performance of the material, and gives it more excellent biological functions by catalyzing the release of nitric oxide. .
Smart Images

Figure CN118976161A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomaterials, and in particular to a metal ion polyphenol coating material, a preparation method and application thereof. Background Art
[0002] In recent years, metal polyphenol networks (MPNs) have attracted increasing attention due to their rapid and simple deposition process on various substrates. This facile deposition method is highly efficient and provides a more flexible option for a wide range of application scenarios. Polyphenols are widely found in plants, such as proanthocyanidins (PC), resveratrol, tannic acid, and catechins. Their unique structure endows them with excellent biological activities such as antioxidant activity, antibacterial activity, pest resistance, anti-obesity activity, anti-thrombotic activity, osteogenic activity, and platelet activity regulation, and therefore has attracted much attention from researchers.
[0003] However, although the materials currently prepared by the method of depositing MPNs on substrates have multiple functions, their comprehensive performance needs to be further improved, such as the ability to promote endothelial cell adhesion and proliferation, and the ability to inhibit smooth muscle cell adhesion and proliferation, which need to be further improved.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a metal ion polyphenol coating material, a preparation method and application thereof, aiming to improve the ability of the material to promote endothelial cell adhesion and proliferation, and at the same time improve the ability of the material to inhibit smooth muscle cell adhesion and proliferation.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a metal ion polyphenol coating material, comprising a substrate and a metal ion polyphenol coating attached to the substrate;
[0008] The metal ion polyphenol coating is formed by the reaction of polyphenol, a first metal ion and a second metal ion; the first metal ion is a strontium ion, and the second metal ion is selected from at least one of a copper ion and a zinc ion.
[0009] In an optional embodiment, the molar ratio of the first metal ion to the second metal ion is (1-100):1; preferably (40-60):1;
[0010] Preferably, the total amount of the first metal ion and the second metal ion accounts for 1% to 50% by mass in the metal ion polyphenol coating.
[0011] In an optional embodiment, the polyphenol is a plant polyphenol containing a polyhydroxyphenol chemical structure;
[0012] Preferably, the polyphenol is selected from at least one of proanthocyanidins, naringenin, resveratrol, tannic acid, quercetin, epicatechin, epicatechin gallate, epigallocatechin, epigallocatechin gallate, chlorogenic acid, ferulic acid, ellagic acid, curcumin and brown algae polyphenols;
[0013] More preferably, the polyphenol is at least one of proanthocyanidins and resveratrol.
[0014] In an optional embodiment, the substrate is selected from at least one of a metal material, an inorganic non-metal material and a polymer material;
[0015] Preferably, the metal material includes stainless steel, iron and its alloys, aluminum and its alloys, magnesium and its alloys, copper and its alloys, titanium and its alloys, zinc and its alloys, uranium and its alloys, and cobalt-based alloys;
[0016] Preferably, the inorganic non-metallic material includes ceramics, glass, titanium dioxide, titanium oxide, titanium nitride, silicon dioxide, silicon carbide, carbon materials, calcium phosphate, aluminosilicate, calcium aluminum bioglass, hydroxyapatite, calcium phosphate silicon nitride, diamond and diamond-like carbon;
[0017] Preferably, the polymer material includes polyester, polyethylene, polyurethane, polyvinyl alcohol, polyvinyl chloride, polypropylene, polycarbonate, carbon copolymer, polyglycolic acid, polymethyl methacrylate, polytetrafluoroethylene, polyoxymethylene, polyvinyl acetate, polystyrene polylactic acid, polylactic acid-glycolic acid copolymer, polyhydroxyalkanoate, polytrimethylene carbonate, polybutylene succinate, polyamide, polydioxanone, polyacrylic acid and its derivatives, polyethylene glycol and its derivatives, polyvinyl alcohol, polycaprolactone and polyurethane, epoxy resin, silicone rubber and silicone gel.
[0018] In a second aspect, the present invention provides a method for preparing the metal ion polyphenol coating material according to any one of the aforementioned embodiments, comprising: immersing a substrate in a mixed solution formed by polyphenol, a first metal ion and a second metal ion for reaction.
[0019] In an optional embodiment, the pH value of the mixed solution is 5-10, the reaction temperature is 10°C-75°C, and the reaction time is 0.5h-24h;
[0020] Preferably, the pH value of the mixed solution is 8-9, the reaction temperature is 15°C-50°C, and the reaction time is 0.5h-20h;
[0021] More preferably, the reaction temperature is 25°C-37°C, and the reaction time is 12h-18h;
[0022] More preferably, the preparation method further comprises: after the reaction is completed, taking out the material for washing and drying.
[0023] In an optional embodiment, the molar ratio of the first metal ion to the polyphenol is (0.1-10):1, and the molar ratio of the second metal ion to the polyphenol is (0.01-0.20):1;
[0024] Preferably, when the second metal ion is a copper ion, the molar ratio of the copper ion to the polyphenol is controlled to be (0.01-0.10):1; when the second metal ion is a zinc ion, the molar ratio of the zinc ion to the polyphenol is controlled to be (0.01-0.20):1;
[0025] Preferably, in the mixed solution, the final concentration of polyphenols is 0.1 mg / mL-50 mg / mL, the final concentration of the first metal ion is 0.01 mg / mL-50 mg / mL; the final concentration of copper ions is 0 μg / mL-300 μg / mL, and the final concentration of zinc ions is 0 μg / mL-600 μg / mL.
[0026] In an optional embodiment, the preparation process of the mixed solution includes: mixing polyphenol, strontium salt, salt containing a second metal ion and a solvent having a pH value that meets the requirements, wherein the salt containing the second metal ion is at least one of a copper salt and a zinc salt;
[0027] Preferably, the strontium salt is selected from at least one of strontium chloride, strontium bromide, strontium iodide, strontium acetate, strontium nitrate and strontium nitrite;
[0028] Preferably, the copper salt is selected from at least one of copper sulfate, copper chloride, cuprous chloride, copper acetate, copper acetate, copper fluoride, copper bromide, cuprous bromide, copper iodide, cuprous iodide, copper citrate, copper tartrate, copper propionate, copper nitrate and ammonia copper ion;
[0029] Preferably, the zinc salt is selected from at least one of zinc sulfate, zinc chloride, zinc nitrate, zinc acetate and zinc fluoride.
[0030] In an optional embodiment, the solvent is a buffer solution with a pH value of 5-10;
[0031] Preferably, the buffer solution is selected from at least one of bicarbonate buffer, PBS buffer, acetic acid / sodium acetate buffer and sodium hydroxide solution;
[0032] More preferably, the buffer solution is a sodium hydroxide solution, and the concentration of the sodium hydroxide solution is 0.001 mol / L-0.01 mol / L.
[0033] In a third aspect, the present invention provides a use of the metal ion polyphenol coating material of any one of the aforementioned embodiments or the metal ion polyphenol coating material prepared by any one of the preparation methods of the aforementioned embodiments in the preparation of implantable medical devices;
[0034] Preferably, the implanted medical device is selected from at least one of a vascular stent, a central venous catheter, a wound dressing and an artificial joint.
[0035] The present invention has the following beneficial effects: a uniform MPNs coating is obtained by depositing polyphenols and metal ions in a one-step method through coordination, cation II and other interactions, and by simultaneously introducing strontium ions and Cu 2+ / Zn 2+ , strontium ion (Sr 2+ ) can participate in bone formation, promote angiogenesis, and also have anti-inflammatory and myocardial repair effects; by introducing Cu 2+ / Zn 2+ , and can also catalyze the release of NO, giving it more excellent performance. The present invention introduces bimetallic materials to improve the ability of the material to promote the adhesion and proliferation of endothelial cells, while improving the ability of the material to inhibit the adhesion and proliferation of smooth muscle cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0037] Figure 1 is the SEM image of Experimental Example 3 on a 316L-SS bracket;
[0038] Figure 2 is the SEM image of Experimental Example 4 on the cobalt-chromium alloy bracket;
[0039] Figure 3 These are scanning electron microscope photos of the anti-platelet adhesion and activation test results of Comparative Example 4 and Example 3;
[0040] Figure 4 These are fluorescent photos of endothelial cell adhesion and proliferation experiments in Comparative Example 1 and Example 1;
[0041] Figure 5 Fluorescence photos of smooth muscle cell adhesion and proliferation experiments in Comparative Example 2 and Example 2;
[0042] Figure 6 The scanning electron microscope photos of the anti-platelet adhesion and activation experimental results of Example 3 and Comparative Example 3;
[0043] Figure 7 Fluorescence photos of the smooth muscle cell adhesion and proliferation experiments in Example 1 and Experimental Example 10;
[0044] Figure 8The thickness of the coating on the 316L-SS bracket of Example 3 and the thickness of the coating on the cobalt-chromium alloy bracket of Example 4. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0046] The embodiment of the present invention provides a method for preparing a metal ion polyphenol coating material, comprising the following steps:
[0047] S1. Preparation of mixed solution
[0048] The prepared mixed solution contains polyphenol, a first metal ion and a second metal ion, wherein the first metal ion is a strontium ion; the second metal ion is at least one selected from copper ions and zinc ions, and the second metal ion may be any one or more of the above.
[0049] In some embodiments, the preparation process of the mixed solution includes: mixing polyphenol, strontium salt, salt containing a second metal ion and a solvent with a pH value that meets the requirements, and stirring evenly. Wherein, the salt containing the second metal ion is at least one of a copper salt and a zinc salt. By using a suitable solvent, the pH value of the mixed solution is 5-10, preferably 8-9. Specifically, the pH value of the mixed solution can be 5, 6, 7, 8, 9, 10, etc., and the strontium salt, copper salt and zinc salt are all soluble salts.
[0050] Further, the polyphenols include plant polyphenols containing polyhydroxyphenol chemical structures, which may include, by way of example but not limitation, at least one of proanthocyanidins, naringenin, resveratrol, tannic acid, quercetin, epicatechin (EC), epicatechin gallate (ECG), epigallocatechin (EGC), epigallocatechin gallate (EGCG), chlorogenic acid, ferulic acid, ellagic acid, curcumin, and brown algae polyphenols, and the polyphenols may be any one or more of the above. In a preferred embodiment, the polyphenols are at least one of proanthocyanidins and resveratrol, and the polyphenols may be any one or more of the above raw materials. By optimizing the types of polyphenols, the ability of the coating to promote endothelial cell adhesion and proliferation can be further enhanced, while the ability of the coating to inhibit smooth muscle cell adhesion and proliferation can be improved.
[0051] Furthermore, the strontium salt is selected from at least one of strontium chloride (SrCl2), strontium bromide (SrBr2), strontium iodide (SrI2), strontium acetate (Sr(CH3COO)2), strontium nitrate (Sr(NO3)2) and strontium nitrite (Sr(NO2)2). The strontium salt can be any one or more of the above, and can be combined with polyphenols in the subsequent reaction process.
[0052] Further, the copper salt is selected from copper sulfate (CuSO4), copper chloride (CuCl2), cuprous chloride (CuCl), copper acetate (Cu(CH3COO)2), copper acetate (Cu(C2H3O2)2), copper fluoride (CuF2), copper bromide (CuBr), cuprous bromide (CuBr2), copper iodide (CuI), cuprous iodide (CuI2), copper citrate (C6H6CuO7), copper tartrate (C4H4CuO6·3H2O), copper propionate (Cu(CO2CH3CH2)2), copper nitrate (Cu(NO3)2) and ammonia copper ion ([Cu(NH3)4] 2+ ), the copper salt may be any one or more of the above soluble copper salts, all of which may be combined with polyphenols in the subsequent reaction process.
[0053] Furthermore, the zinc salt is selected from at least one of zinc sulfate (ZnSO4), zinc chloride (ZnCl2), zinc nitrate (Zn(NO3)2), zinc acetate (Zn(C2HO2)2), and zinc fluoride (ZnF2). The zinc salt can be any one or more of the above. The above soluble zinc salts can all combine with polyphenols during the reaction process, and the reaction is more complete.
[0054] In some embodiments, the molar ratio of the first metal ion to the polyphenol is (0.1-10):1, and the molar ratio of the second metal ion to the polyphenol is (0.01-0.20):1. By further regulating the dosage of the first metal ion and the second metal ion, the molar ratio of the two on the surface of the substrate after deposition is controlled, thereby improving the ability of the coating to promote endothelial cell adhesion and proliferation, and at the same time improving the ability of the coating to inhibit smooth muscle cell adhesion and proliferation. When the second metal ion is a copper ion, the molar ratio of the copper ion to the polyphenol is controlled to be (0.01-0.10):1; when the second metal ion is a zinc ion, the molar ratio of the zinc ion to the polyphenol is controlled to be (0.01-0.20):1. The type of the second metal ion is different, and the dosage is also adjusted within the above range. If the dosage of each metal ion exceeds the above range, it will lead to a decrease in the overall performance of the coating.
[0055] Specifically, the molar ratio of the first metal ion and the polyphenol can be 0.1:1, 0.5:1, 1.0:1, 2.0:1, 3.0:1, 4.0:1, 5.0:1, 6.0:1, 7.0:1, 8.0:1, 9.0:1, 10.0:1, etc.; the molar ratio of the second metal ion and the polyphenol can be 0.01:1, 0.03:1, 0.05:1, 0.08:1, 0.10:1, 0.13:1, 0.15:1, 0.18:1, 0.20:1, etc.
[0056] In some embodiments, in the mixed solution, the final concentration of polyphenols is 0.1 mg / mL-50 mg / mL, such as 0.1 mg / mL, 0.5 mg / mL, 1.0 mg / mL, 10.0 mg / mL, 20.0 mg / mL, 30.0 mg / mL, 40.0 mg / mL, 50.0 mg / mL, etc. The final concentration of the first metal ion is 0.01 mg / mL-50 mg / mL, such as 0.01 mg / mL, 0.05 mg / mL, 0.10 mg / mL, 1.00 mg / mL, 10.00 mg / mL, 20.00 mg / mL, 30.00 mg / mL, 40.00 mg / mL, 50.00 mg / mL, etc. The final concentration of copper ions is 0 μg / mL-300 μg / mL, such as 0 μg / mL, 10 μg / mL, 50 μg / mL, 100 μg / mL, 150 μg / mL, 200 μg / mL, 250 μg / mL, 300 μg / mL, etc. The final concentration of zinc ions is 0 μg / mL-600 μg / mL, such as 0 μg / mL, 10 μg / mL, 50 μg / mL, 100 μg / mL, 150 μg / mL, 200 μg / mL, 250 μg / mL, 300 μg / mL, 350 μg / mL, 400 μg / mL, 450 μg / mL, 500 μg / mL, 550 μg / mL, 600 μg / mL, etc. However, copper ions and zinc ions are not 0 at the same time, and at least one of them must be contained. By controlling the above preferred molar ratio and concentration scheme, the two polyphenols, Sr 2+ and Cu 2+ / Zn 2+ The specific properties of the polyphenols can form an optimal metal ion coating.
[0057] In some embodiments, the solvent is a buffer solution with a pH value of 5-10, so that the pH value of the mixed solution meets the requirements, such as the pH value of the buffer solution can be 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, etc. The buffer solution is selected from at least one of a bicarbonate buffer, a PBS buffer, an acetic acid / sodium acetate buffer solution, and a sodium hydroxide solution, and the buffer solution can be any one of the above.
[0058] In a preferred embodiment, the buffer solution is a sodium hydroxide solution, and the concentration of the sodium hydroxide solution is 0.001mol / L-0.01mol / L, such as 0.001mol / L, 0.003mol / L, 0.005mol / L, 0.008mol / L, 0.010mol / L, etc.
[0059] It should be noted that the raw materials used in the embodiments of the present invention are all common substances or extracts, which are non-toxic, harmless, have good biocompatibility, and have stable chemical structures. After forming the coating, the physiological functions of the various substances are not affected, and they work synergistically to exert physiological effects.
[0060] S2. Forming coating
[0061] The substrate is immersed in a mixed solution formed by polyphenol, the first metal ion and the second metal ion, and stirred or gently shaken to be uniform, and reacted for a period of time. In the process of forming the metal ion polyphenol coating, the polyphenol and Sr 2+ , Cu 2+ / Zn 2+ A uniform MPNs coating is obtained by one-step deposition through coordination and cation π interaction. The coating is non-biotoxic and can maintain the original physiological functions of polyphenols and metal ions. 2+ / Zn 2+ , and can also catalyze the release of NO, giving it more excellent properties.
[0062] In some embodiments, the reaction temperature is 10°C-75°C, such as 10°C, 15°C, 20°C, 25°C, 30°C, 37°C, 40°C, 50°C, 75°C, etc.; the reaction time is 0.5h-24h, such as 0.5h, 1h, 6h, 12h, 15h, 18h, 20h, 24h, etc. In a preferred embodiment, the reaction temperature is 15°C-50°C, and the reaction time is 0.5h-20h; in a more preferred embodiment, the reaction temperature is 25°C-37°C, and the reaction time is 12h-18h.
[0063] It should be noted that by regulating the reaction temperature and time, the molar ratio of metal ions and polyphenols is regulated, and then the surface structure and coating thickness are regulated. The formed metal polyphenol functionalized coating can quickly form a film on the surface of metal, non-metal, polymer and other materials, and the preparation method is simple and easy. The multifunctional metal ion polyphenol coating formed by the method provided by the embodiment of the present invention has a broad spectrum modification characteristic, and its excellent physical and chemical structural stability is not affected by the substrate material, and has broad application prospects in the field of biomaterial technology.
[0064] In some embodiments, the substrate is selected from at least one of a metal material, an inorganic non-metallic material, and a polymer material. The substrate can be any one or more of the above. The above substrates are all suitable for the preparation method provided in the embodiments of the present invention. A suitable substrate can be selected for reaction according to the different uses of the material.
[0065] Furthermore, the metal materials include stainless steel, iron and its alloys, aluminum and its alloys, magnesium and its alloys, copper and its alloys, titanium and its alloys, zinc and its alloys, uranium and its alloys, and cobalt-based alloys. The metal materials include the above materials, and the substrate can be selected from any one or several of the above materials.
[0066] Furthermore, inorganic non-metallic materials include ceramics, glass, titanium dioxide, titanium oxide, titanium nitride, silicon dioxide, silicon carbide, carbon materials, calcium phosphate, aluminosilicate, calcium aluminum bioglass, hydroxyapatite, calcium phosphate silicon nitride, diamond and diamond-like carbon. Inorganic non-metallic materials include the above, and the substrate can be selected from any one or several of the above-mentioned inorganic non-metallic materials.
[0067] Further, the polymer material includes polyester, polyethylene, polyurethane, polyvinyl alcohol, polyvinyl chloride, polypropylene, polycarbonate, carbon copolymer, polyglycolic acid, polymethyl methacrylate, polytetrafluoroethylene, polyoxymethylene, polyvinyl acetate, polystyrene polylactic acid, polylactic acid-glycolic acid copolymer, polyhydroxyalkanoate, polytrimethylene carbonate, polybutylene succinate, polyamide, polydioxanone, polyacrylic acid and its derivatives, polyethylene glycol and its derivatives, polyvinyl alcohol, polycaprolactone and polyurethane, epoxy resin, silicone rubber and silicone gel. The polymer material includes the above several, and the substrate can select any one or several of them from the above several polymer materials.
[0068] S3, post-processing
[0069] After the S2 reaction is completed, the material is taken out for cleaning and drying. The unbound ions on the surface are removed by cleaning, and the pure product is obtained after drying to remove the cleaning solvent.
[0070] Specifically, the surface of the substrate can be washed with distilled water for 3 times, each time for 3 minutes, to effectively remove the undeposited reactants on the surface. After washing, the substrate is placed in an oven for drying to obtain a multifunctional metal ion polyphenol coating.
[0071] The embodiment of the present invention also provides a metal ion polyphenol coating material, including a substrate and a metal ion polyphenol coating attached to the substrate; wherein the metal ion polyphenol coating is formed by the reaction of polyphenol, a first metal ion and a second metal ion; the first metal ion is a strontium ion, the second metal ion is selected from at least one of a copper ion and a zinc ion, and the second metal ion can be any one or more of the above. The metal ion polyphenol coating material can be prepared by the above preparation method, and the specific preparation process is not repeated here.
[0072] It should be noted that strontium ions (Sr 2+ ) has a very important physiological role, especially in the skeletal system and vascular biology, such as participating in bone formation, promoting angiogenesis, anti-inflammation, promoting myocardial repair, etc. In addition, copper ions (Cu 2+ ) and zinc ions (Zn 2+ ) participate in the activity of a variety of enzymes that play key roles in redox reactions and free radical scavenging. More importantly, Cu 2+ and Zn 2+ It exhibits catalytic activity similar to that of glutathione reductase, catalyzing the decomposition of S-sulfhydryl compounds in the blood to produce nitric oxide (NO), thereby playing an important cardiovascular protective role such as relaxing blood vessels, resisting platelet aggregation, inhibiting smooth muscle proliferation, and protecting endothelial cells.
[0073] In some embodiments, the molar ratio of the first metal ion to the second metal ion is (1-100):1, such as 1:1, 1:5, 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, etc., preferably (40-60):1. The total amount of the first metal ion and the second metal ion in the metal ion polyphenol coating accounts for 1%-50% by weight (such as 1%, 10%, 20%, 30%, 40%, 50%, etc.). It is appropriate to control the mass ratio and molar ratio of the first metal ion and the second metal ion within the above range, which can further enhance the ability of the coating to promote endothelial cell adhesion and proliferation, and at the same time enhance the ability of the coating to inhibit smooth muscle cell adhesion and proliferation.
[0074] The metal ion polyphenol coating material provided in the embodiment of the present invention can be used in the preparation of implantable medical devices, and can be used to prepare the surface layer of implantable medical devices. It has the effects of protecting the cardiovascular system, promoting bone regeneration, anti-inflammatory, antibacterial, and anti-thrombotic. It can also catalyze the release of NO, giving it more excellent properties.
[0075] Furthermore, the implanted medical device is selected from at least one of a vascular stent, a central venous catheter, a wound dressing and an artificial joint, and the implanted medical device may be any one or more of the above.
[0076] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0077] Example 1
[0078] This embodiment provides a method for preparing a metal ion polyphenol coating material, comprising the following steps:
[0079] (1) The silicone rubber substrate was thoroughly cleaned with distilled water, and then ultrasonically cleaned with anhydrous ethanol for three times, each time for 5 minutes, and then dried in an oven for later use.
[0080] (2) Proanthocyanidin (purchased from damas-beta, model number p1523063) and SrCl2 were mixed in distilled water at a molar ratio of 1:2, and ultrasonicated for 10 minutes to fully dissolve the proanthocyanidin to obtain a mixed solution A with a pH of 8. Proanthocyanidin and CuCl2 were then mixed in distilled water at a molar ratio of 1:0.03 to obtain a mixed solution B with a pH of 8. Then, solution A and solution B were mixed to obtain a final concentration of proanthocyanidin of 2.5 mg / mL, a final concentration of SrCl2 of 2.5 mg / mL, and a final concentration of CuCl2 of 25 ug / mL. (After conversion, the molar ratio of proanthocyanidin, strontium ion, and copper ion is 5.337:15.76:0.1859)
[0081] (3) Immerse the silicone rubber to be used in the above mixed solution and gently mix it. Then place it in a constant temperature box at 25°C for 12 hours to perform reaction deposition.
[0082] (4) After the reaction is completed, the silicone rubber is taken out and gently rinsed with distilled water for three times. The surface water is absorbed from the side with filter paper and then dried in an oven to obtain a metal ion polyphenol coating sample with multifunctionality.
[0083] Example 2
[0084] This embodiment is basically the same as embodiment 1, except that the polyphenols are replaced by an equal amount of tannic acid instead of proanthocyanidins, and the molar ratio of polyphenols, strontium ions, and copper ions is kept unchanged.
[0085] Example 3
[0086] This embodiment provides a method for preparing a metal ion polyphenol coating material, comprising the following steps:
[0087] (1) The 316L stainless steel substrate was thoroughly cleaned with distilled water, then ultrasonically cleaned with anhydrous ethanol three times, each time for 5 minutes, and then ultrasonically cleaned with acetone three times, and then dried in an oven for later use.
[0088] (2) Resveratrol (purchased from Aladdin, model number R40871) and SrCl2 were mixed in distilled water at a molar ratio of 1:1, and ultrasonicated for 10 minutes to fully dissolve resveratrol to obtain a mixed solution A with a pH of 9. Resveratrol and ZnCl2 were then mixed in distilled water at a molar ratio of 1:0.05 to obtain a mixed solution B with a pH of 9. Then, solution A and solution B were mixed to obtain a final concentration of resveratrol of 3 mg / mL, a final concentration of SrCl2 of 3 mg / mL, and a final concentration of ZnCl2 of 50 ug / mL. (After conversion, the molar ratio of resveratrol, strontium ion, and zinc ion is 13.144:18.913:0.3668)
[0089] (3) Immerse the 316L stainless steel substrate to be used in the above mixed solution, gently mix it, and then place it in a constant temperature box at 37°C for 12 hours to perform reaction deposition.
[0090] (4) After the reaction is completed, the 316L stainless steel substrate is taken out and gently rinsed with distilled water three times. The surface water is absorbed from the side with filter paper and then dried in an oven to obtain a metal ion polyphenol coating sample with multifunctionality.
[0091] Example 4
[0092] This embodiment is basically the same as Embodiment 3, except that the substrate is replaced with a cobalt-chromium alloy.
[0093] Example 5
[0094] This example is basically the same as Example 3, except that the polyphenols are replaced with an equal molar amount of ellagic acid (purchased from Aladdin, model number E102710), i.e., the molar amount of polyphenols in the total mixed solution obtained in step (2) remains unchanged.
[0095] Example 6
[0096] This embodiment provides a method for preparing a metal ion polyphenol coating material, comprising the following steps:
[0097] (1) The titanium dioxide sheet was thoroughly cleaned with distilled water, then ultrasonically cleaned with anhydrous ethanol for three times, each time for 5 minutes, then ultrasonically cleaned with acetone for three times, and dried in an oven for later use.
[0098] (2) Gallic acid (purchased from Aladdin, model number G329710) and SrCl2 were mixed in distilled water at a molar ratio of 1:1, and ultrasonicated for 10 minutes to fully dissolve the gallic acid to obtain a mixed solution A with a pH of 8.5. Gallic acid and CuCl2 were then mixed in distilled water at a molar ratio of 1:0.03 to obtain a mixed solution B with a pH of 8.5. Then, liquid A and liquid B were mixed to obtain a final concentration of gallic acid of 3 mg / mL, a final concentration of SrCl2 of 3 mg / mL, and a final concentration of CuCl2 of 25 ug / mL. (After conversion, the molar ratio of gallic acid, strontium ion, and copper ion is 1:1.072:0.0105)
[0099] (3) Immerse the titanium dioxide sheet to be used in the mixed solution and gently mix it. Then place it in a constant temperature box at 25°C for 14 hours to perform reaction deposition.
[0100] (4) After the reaction is completed, the titanium dioxide sheet is taken out and gently rinsed with distilled water for three times. The water on the surface is absorbed from the side with filter paper and then dried in an oven to obtain a metal ion polyphenol coating sample with multifunctionality.
[0101] Example 7
[0102] This embodiment is basically the same as embodiment 6, except that the pH value of the mixed solution is 10 (adjusted by sodium hydroxide solution), the reaction temperature is 37° C., and the reaction time is 20 h.
[0103] Example 8
[0104] This example is basically the same as Example 6, except that the final concentration of CuCl2 is 100ug / mL. (After conversion, the molar ratio of gallic acid, strontium ion, and copper ion is 1:1.072:0.0421)
[0105] Example 9
[0106] This embodiment is substantially the same as embodiment 6, except that the polyphenol is brown algae polyphenol.
[0107] Example 10
[0108] The only difference between this embodiment and embodiment 1 is that the content of each component in the total mixed solution prepared in step (2) is changed so that the molar ratio of proanthocyanidins, strontium ions and copper ions is 30:80:1.
[0109] Embodiment 11
[0110] The only difference between this embodiment and embodiment 1 is that the content of each component in the total mixed solution prepared in step (2) is changed so that the molar ratio of proanthocyanidins, strontium ions and copper ions is 50:50:1.
[0111] Example 12
[0112] The only difference between this embodiment and embodiment 1 is that the copper ions in step (2) are replaced by an equimolar amount of zinc ions.
[0113] Comparative Example 1
[0114] The difference between this comparative example and Example 1 is that no CuCl2 is added, so that the molar amount of strontium ions added to the total mixed solution obtained in step (2) is equal to the total amount of copper ions and strontium ions added in Example 1.
[0115] Comparative Example 2
[0116] The only difference between this comparative example and Example 2 is that SrCl2 is not added, so that the molar amount of copper ions added to the total mixed solution obtained in step (2) is equal to the total amount of copper ions and strontium ions added in Example 2.
[0117] Comparative Example 3
[0118] The difference between this comparative example and Example 3 is that the pH of the distilled water is adjusted to 10 and the temperature is adjusted to 50°C.
[0119] The substrate was 316L SS, and the final concentrations of resveratrol, SrCl2, and ZnCl2 were controlled to be 3 mg / mL, 3 mg / mL, and 50 ug / mL. The mixture was reacted at 37°C for 12 hours, washed three times with distilled water, dried in an oven, and dried at 37°C.
[0120] Comparative Example 4
[0121] The only difference between this comparative example and Example 3 is that SrCl2 and ZnCl2 are not added.
[0122] The substrate was 316L SS, the concentration of resveratrol was controlled to be 3 mg / mL, the mixture was reacted at 37°C for 12 h, washed three times with distilled water, dried in an oven, and placed in a dry environment at 37°C for later use.
[0123] Test Example 1
[0124] The microscopic morphology of the surface coating of the medical 316L SS stent prepared in Example 3 is as follows: Figure 1 As shown, it can be seen that the coating maintains good adhesion on the surface of the stent and is deposited evenly without obvious cracking, proving that the coating can fully adapt to the deformation of the stent during expansion and compression.
[0125] Test Example 2
[0126] The microscopic morphology of the surface coating of the medical cobalt-chromium alloy vascular stent prepared in Example 4 was tested. The results are as follows: Figure 2As shown, it can be seen that the coating maintains good adhesion on the surface of the stent and is deposited evenly without obvious cracking, proving that the coating can fully adapt to the deformation of the stent during expansion and compression.
[0127] Test Example 3
[0128] Platelet adhesion and activation experiments were performed using the materials obtained in Example 3 and Comparative Example 4. The results are as follows: Figure 3 shown.
[0129] Experimental methods:
[0130] (1) The materials prepared in Example 3 and Comparative Example 4 were compared using a static platelet adhesion experiment. First, whole blood from healthy New Zealand rabbits was collected using a vacuum negative pressure tube containing sodium citrate anticoagulant. Platelet-rich plasma (PRP) was collected by centrifugation at 1500 rpm for 15 min.
[0131] (2) Add 200 μL of fresh PRP to the surfaces of the two coatings and incubate at 37°C for 30 min. Wash the non-adherent platelets with saline, fix them in 2.5% glutaraldehyde solution for 12 h, dehydrate them with ethanol, and observe the morphology and number of platelets using a scanning electron microscope.
[0132] from Figure 3 It can be seen that the number of platelets adhered and the degree of activation on the surface of Example 3 are significantly less than those of Comparative Example 4, showing excellent anti-platelet adhesion and activation functions, indicating that Example 3 has better blood compatibility.
[0133] Test Example 4
[0134] The materials obtained in Example 1 and Comparative Example 1 were subjected to endothelial cell adhesion and proliferation experiments. The fluorescence photos are shown in FIG. Figure 4 shown.
[0135] Test method: Endothelial cells were planted on the surface of the materials prepared in Example 1 and Comparative Example 1, and photographed under an inverted fluorescence microscope after being cultured for 24 hours and 72 hours, respectively.
[0136] from Figure 4 It can be seen that the number of endothelial cells adhered to the surface of Example 1 is significantly higher than that of Comparative Example 1, and the proliferation is also more excellent, indicating that Example 1 has a more significant ability to promote endothelial cell adhesion and proliferation.
[0137] Test Example 5
[0138] The materials obtained in Test Example 2 and Comparative Example 2 were subjected to smooth muscle cell adhesion and proliferation experiments. The fluorescence photos are shown in FIG. Figure 5 shown.
[0139] Test method: Smooth muscle cells were planted on the surface of the materials prepared in Example 2 and Comparative Example 2, and images were taken using an inverted fluorescence microscope after culturing for 24 hours and 72 hours, respectively. Figure 5 It can be seen that the number of smooth muscle cells adhered to the surface of Example 2 is significantly lower than that of Comparative Example 2, and the proliferation is also inhibited, indicating that Example 2 has a more significant ability to inhibit the adhesion and proliferation of smooth muscle cells.
[0140] It can be seen that copper ions have the effect of inhibiting the adhesion and proliferation of smooth muscle cells, while strontium ions and copper ions have a synergistic effect and can enhance the ability to inhibit the adhesion and proliferation of smooth muscle cells.
[0141] Test Example 6
[0142] The microscopic morphology of the coating prepared on the substrate of 316L SS surface was tested in Example 3 and Comparative Example 3. The results are as follows: Figure 6 It can be seen that the coating of Experimental Example 3 is more uniform, denser, thicker, and has a more complete coating coverage than that of Comparative Example 3, which proves that the coating process of Example 3 is better and more suitable for surface modification of 316L SS substrate.
[0143] Test Example 7
[0144] The materials obtained in Example 1 and Experimental Example 10 were subjected to smooth muscle cell adhesion and proliferation experiments. The fluorescence photos are shown in FIG. Figure 7 shown.
[0145] Test method: Smooth muscle cells were planted on the surface of the materials prepared in Example 1 and Experimental Example 10, and images were taken using an inverted fluorescence microscope after culturing for 24 hours and 72 hours, respectively. Figure 7 It can be seen that the number of smooth muscle cells adhered to the surface of Example 1 is significantly lower than that of Experimental Example 10, and the proliferation is also inhibited, indicating that Example 1 has a more significant ability to inhibit the adhesion and proliferation of smooth muscle cells.
[0146] Test Example 8
[0147] The thickness of the surface coating of the medical 316L SS vascular stent prepared in Example 3 and the surface coating of the medical cobalt-chromium alloy vascular stent prepared in Example 4 were tested. The results are as follows: Figure 8 As shown in the figure, it can be seen that the thickness of the coating on the cobalt-chromium alloy stent is significantly higher than that on the 316L SS vascular stent, indicating that the coating has better bonding with the cobalt-chromium alloy substrate.
[0148] By comparing the experimental results of the embodiments and comparative examples, it can be found that the various modified materials in the embodiments of the present application all have corresponding functional performances. According to the application scenario and scope of use, suitable polyphenols and metal ions with anti-inflammatory activity, antibacterial activity, antioxidant activity, etc. can be selected to form a metal phenolamine coating. By controlling the type of polyphenols, the concentration of polyphenols and metal ions, and the coating reaction time, an adjustable and controllable metal ion polyphenol coating for multiple scenarios can be achieved.
[0149] In summary, the present invention utilizes polyphenols and metal ions to deposit uniform MPNs coatings through coordination, cation II and other interactions in one step, and simultaneously introduces strontium ions and Cu 2+ / Zn 2+ . The present invention prepares a multifunctional metal ion polyphenol coating through a one-step method, which can have the characteristics of broad-spectrum modification, is independent of the substrate material, and has broad application prospects in the field of biomaterial technology. In addition, the functional coating also has the characteristics of good physical and chemical stability, and can maintain stable and good effects in various environments. The functional coating preparation method of the present invention is simple, low-cost, and easy to mass produce and apply.
[0150] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A metal ion polyphenol coating material, characterized in that: It includes a substrate and a metal ion polyphenol coating attached to the substrate; The metal ion polyphenol coating is formed by the reaction of polyphenol, a first metal ion and a second metal ion; the first metal ion is a strontium ion, and the second metal ion is selected from at least one of a copper ion and a zinc ion.
2. The metal ion polyphenol coating material according to claim 1, characterized in that: The molar ratio of the first metal ion to the second metal ion is (1-100):1; preferably (40-60):1; Preferably, the total amount of the first metal ions and the second metal ions in the metal ion polyphenol coating accounts for 1% to 50% by mass.
3. The metal ion polyphenol coating material according to claim 1, characterized in that: The polyphenols are plant polyphenols containing a polyhydroxyphenol chemical structure; Preferably, the polyphenol is selected from at least one of proanthocyanidins, naringenin, resveratrol, tannic acid, quercetin, epicatechin, epicatechin gallate, epigallocatechin, epigallocatechin gallate, chlorogenic acid, ferulic acid, ellagic acid, curcumin and brown algae polyphenols; More preferably, the polyphenol is at least one of proanthocyanidins and resveratrol.
4. The metal ion polyphenol coating material according to claim 1, characterized in that: The substrate is selected from at least one of a metal material, an inorganic non-metal material and a polymer material; Preferably, the metal material includes stainless steel, iron and its alloys, aluminum and its alloys, magnesium and its alloys, copper and its alloys, titanium and its alloys, zinc and its alloys, uranium and its alloys, and cobalt-based alloys; Preferably, the inorganic non-metallic material includes ceramics, glass, titanium dioxide, titanium oxide, titanium nitride, silicon dioxide, silicon carbide, carbon materials, calcium phosphate, aluminosilicate, calcium aluminum bioglass, hydroxyapatite, calcium phosphate silicon nitride, diamond and diamond-like carbon; Preferably, the polymer material includes polyester, polyethylene, polyurethane, polyvinyl alcohol, polyvinyl chloride, polypropylene, polycarbonate, carbon copolymer, polyglycolic acid, polymethyl methacrylate, polytetrafluoroethylene, polyoxymethylene, polyvinyl acetate, polystyrene polylactic acid, polylactic acid-glycolic acid copolymer, polyhydroxyalkanoate, polytrimethylene carbonate, polybutylene succinate, polyamide, polydioxanone, polyacrylic acid and its derivatives, polyethylene glycol and its derivatives, polyvinyl alcohol, polycaprolactone and polyurethane, epoxy resin, silicone rubber and silicone gel.
5. A method for preparing the metal ion polyphenol coating material according to any one of claims 1 to 4, characterized in that: include: The substrate is immersed in a mixed solution formed by the polyphenol, the first metal ions and the second metal ions for reaction.
6. The preparation method according to claim 5, characterized in that: The pH value of the mixed solution is 5-10, the reaction temperature is 10°C-75°C, and the reaction time is 0.5h-24h; Preferably, the pH value of the mixed solution is 8-9, the reaction temperature is 15°C-50°C, and the reaction time is 0.5h-20h; More preferably, the reaction temperature is 25°C-37°C, and the reaction time is 12h-18h; More preferably, the preparation method further comprises: after the reaction is completed, taking out the material for washing and drying.
7. The preparation method according to claim 5, characterized in that: The molar ratio of the first metal ion to the polyphenol is (0.1-10):1, and the molar ratio of the second metal ion to the polyphenol is (0.01-0.20):1; Preferably, when the second metal ion is a copper ion, the molar ratio of the copper ion to the polyphenol is controlled to be (0.01-0.10):1; when the second metal ion is a zinc ion, the molar ratio of the zinc ion to the polyphenol is controlled to be (0.01-0.20):1; Preferably, in the mixed solution, the final concentration of the polyphenol is 0.1 mg / mL-50 mg / mL, the final concentration of the first metal ion is 0.01 mg / mL-50 mg / mL; the final concentration of the copper ion is 0 μg / mL-300 μg / mL, and the final concentration of the zinc ion is 0 μg / mL-600 μg / mL.
8. The preparation method according to claim 7, characterized in that: The preparation process of the mixed solution comprises: mixing the polyphenol, strontium salt, salt containing the second metal ion and a solvent with a pH value that meets the requirements, wherein the salt containing the second metal ion is at least one of copper salt and zinc salt; Preferably, the strontium salt is selected from at least one of strontium chloride, strontium bromide, strontium iodide, strontium acetate, strontium nitrate and strontium nitrite; Preferably, the copper salt is selected from at least one of copper sulfate, copper chloride, cuprous chloride, copper acetate, copper acetate, copper fluoride, copper bromide, cuprous bromide, copper iodide, cuprous iodide, copper citrate, copper tartrate, copper propionate, copper nitrate and ammonia copper ion; Preferably, the zinc salt is selected from at least one of zinc sulfate, zinc chloride, zinc nitrate, zinc acetate and zinc fluoride.
9. The preparation method according to claim 8, characterized in that: The solvent is a buffer solution with a pH value of 5-10; Preferably, the buffer solution is selected from at least one of bicarbonate buffer, PBS buffer, acetic acid / sodium acetate buffer and sodium hydroxide solution; More preferably, the buffer solution is a sodium hydroxide solution, and the concentration of the sodium hydroxide solution is 0.001 mol / L-0.01 mol / L.
10. Use of the metal ion polyphenol coating material according to any one of claims 1 to 4 or the metal ion polyphenol coating material prepared by the preparation method according to any one of claims 5 to 9 in the preparation of implantable medical devices; Preferably, the implanted medical device is selected from at least one of a vascular stent, a central venous catheter, a wound dressing and an artificial joint.
Citation Information
Cited By
Swim bladder-based bioactive patch for rotator cuff tendon repair and preparation method of swim bladder-based bioactive patch
CN120393121A
New application of organic-inorganic ion co-intercalation LDH composite coating modified by tannic acid-copper ion complex
CN121003734A
Coating-modified high-molecular polymer porous scaffold as well as preparation method and application thereof
CN121177574A
Novel metal-polyphenol microspheres as well as preparation method and application thereof
CN121265809A
Injectable bone repair material containing bioactive glass and preparation method thereof
CN121944224A