Preparation method and application of steel slag modified and reconstructed CO2-absorbing adsorption material

By using a process of mixed flux melting, acid leaching, and selective precipitation, a high-efficiency CO2 adsorption material was prepared, which solved the problem of low conversion rate of calcium oxide component in steel slag and achieved the effect of efficient CO2 fixation.

CN118976458APending Publication Date: 2024-11-19JIANGSU UNIV OF SCI & TECH

Patent Information

Application Number
CN202411047190.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the current process of CO2 adsorption, the conversion rate of calcium oxide component in steel slag is low, the amount of CO2 fixed per unit of steel slag is insufficient, and the utilization rate of steel slag is low, resulting in environmental pollution and resource waste.

Method used

A highly efficient CO2 adsorbent material was prepared by using a process of mixed flux melting, acid leaching, selective precipitation and drying, by adding flux to accelerate the dissolution rate of steel slag, using hydrofluoric acid to enhance the separation of calcium and silicon ions, and selectively precipitating calcium-containing ions.

Benefits of technology

It improved the conversion rate of calcium oxide components and the amount of CO2 fixed per unit of steel slag, shortened the reaction time, enhanced the carbon fixation efficiency of steel slag, and achieved the effect of highly efficient CO2 adsorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976458A_ABST
    Figure CN118976458A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a steel slag modified and reconstructed CO2-absorbing adsorbing material in the fields of greenhouse gas CO2 emission reduction, steel slag resource utilization and CO2 immobilization. Original steel slag and a fluxing agent are mixed, molten and cooled to obtain molten steel slag, hydrochloric acid is added into the molten steel slag to completely dissolve the molten steel slag to obtain a dissolved solution, and the dissolved solution is added into a water bath to obtain the CO2-absorbing adsorbing material. Hydrofluoric acid is added into the dissolving solution, then perchloric acid is added into the reaction solution, and a mixed solution is obtained; adding alkali liquor into the mixed solution to selectively adjust the pH value to 3-4 and 9-11, performing selective fractional precipitation to obtain filter residues, washing the filter residues with water, and evaporating water vapor to prepare the required CO2 adsorption material for absorbing CO2 gas; the solubility of the steel slag and the leaching rate of the Ca element are improved from the perspective of not adjusting the mineral composition of the steel slag, the carbon sequestration efficiency is high, the reaction time is short, the conversion rate of calcium oxide components is high, and the amount of CO2 immobilized by unit steel slag is large.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of greenhouse gas CO2 emission reduction, steel slag resource utilization and CO2 fixation, and particularly relates to the preparation of an adsorption material for efficiently absorbing CO2 by modifying and reconstructing steel slag. Background Art

[0002] Steel slag is a major solid waste produced during the steelmaking process, and its output is about 10-15% of the crude steel. At present, the utilization rate of steel slag is low, and a large amount of steel slag cannot be effectively utilized and is piled up in an open-air environment, which not only occupies a large amount of land but also pollutes the environment. Steel slag contains 40%-55% CaO, which has a good adsorption capacity for CO2. Therefore, if steel slag can be used to adsorb CO2 and stored for a long time in a stable carbonate form, it can not only greatly improve the resource utilization rate of steel slag, but also achieve the goal of carbon reduction in the steel industry.

[0003] Steel slag is not easy to completely dissolve in acid solution, and the CaO content actually participating in the reaction during the carbonation of steel slag is not high. Therefore, steel slag is not directly used to adsorb CO2 in industry. Instead, the steel slag is first modified and reformed into more active CaO, and then CO2 is adsorbed. Therefore, many studies focus on the carbonation of Ca element in steel slag. There are direct carbonation and indirect carbonation for the carbonation of Ca element in steel slag. Direct liquid phase carbonation refers to the carbonation reaction of calcium-containing minerals in steel slag directly with CO2 in a liquid phase environment to form carbonate precipitates. Indirect carbonation is to divide the carbonation reaction into two steps: leaching and precipitation. For indirect carbonation, the main focus is on how to maximize the Ca 2+ Acetic acid (CH3COOH) and ammonium chloride (NH4Cl) are commonly used leaching agents and are widely used in the leaching process of indirect carbonation of steel slag. They can selectively leach Ca 2+ Comparing the results of leaching steel slag with CH3COOH and NH4Cl as leaching agents, it was found that CH3COOH had a stronger effect on Ca 2+ The leaching rate is higher than that of NH4Cl. For example, a method for fixing CO2 and digesting free calcium oxide in steel slag powder is disclosed in the document with Chinese patent publication number CN101851071A. The process is to first soak the converter slag in water, then add it to the grinding mill, and at the same time introduce waste hot flue gas (150-180°C) containing CO2, and then dry the slag powder; this method mainly couples the steel slag ball milling with the carbonation reaction, that is, mechanically stripping off the unreacted calcium oxide wrapped on the surface of calcium carbonate.

[0004] For the carbonation of steel slag, acidic reagents are generally used to completely leach and dissolve the steel slag and the Ca element therein, and the reaction is promoted by acid solubility, reaction time, temperature, stirring rate, steel slag particle size and liquid-solid ratio. However, although this method can improve the solubility of steel slag, steel slag is not easy to completely dissolve in acid solution and the low content of free calcium oxide in steel slag limits its carbon fixation potential; in addition, when steel slag is carbonated, the calcium oxide component is partially fixed, and the calcium carbonate formed by reaction with CO2 tends to cover the surface of unreacted calcium oxide, thereby inhibiting further carbonation. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings of the existing steel slag utilization and to propose a preparation method and application of a steel slag modified and reconstructed adsorption material for absorbing CO2 with high calcium oxide component conversion rate and large amount of CO2 fixed per unit steel slag.

[0006] To achieve the above object, the technical solution adopted by the method for preparing a CO2 absorbing adsorbent material by modifying and reconstructing steel slag in the present invention comprises the following steps:

[0007] Step 1): mixing the original steel slag with a flux, melting the mixture at a temperature of 800 to 1400° C., and cooling the mixture to obtain molten steel slag;

[0008] Step 2): adding hydrochloric acid to the molten slag to completely dissolve it to obtain a solution, adding hydrofluoric acid to the solution, reacting at a temperature of 90 to 400° C. to obtain a reaction solution, then adding perchloric acid to the reaction solution, stirring at a constant temperature of 90 to 400° C., stopping stirring and cooling to room temperature to obtain a mixed solution;

[0009] Step 3): adding alkali solution to the mixed solution to selectively adjust the pH value to 3-4 and 9-11, selectively precipitating step by step, so that iron and calcium ions are precipitated step by step to obtain filter residues, and washing the filter residues to obtain initial adsorptive materials;

[0010] Step 4): The initial adsorbent material is fully evaporated to produce the desired CO2 adsorbent material.

[0011] Furthermore, in step 1), the flux is one or a combination of lithium tetraborate, lithium metaborate, sodium carbonate, boric acid, and sodium peroxide, the mass ratio of the original steel slag to the flux is 1:1-20, and the melting time is 5-120 min.

[0012] Furthermore, in step 2), the molten steel slag is first ground into powder with a particle size not exceeding 0.2 mm, and then hydrochloric acid with a concentration of 20% to 40wt% is added.

[0013] Furthermore, in step 2), the solid-liquid ratio of the molten steel slag to hydrochloric acid is 1:3-20; the concentration of the hydrofluoric acid is 20%-50.0wt%, and the mass of the hydrofluoric acid added is 1-2.6 times the mass of the original steel slag; the concentration of the perchloric acid is 20%-50.0wt%, and the mass of the chloric acid added is 0.5-1.3 times the mass of the original steel slag; the stirring speed is 30-180r / min, and the stirring time is 20-180min.

[0014] Furthermore, in step 3), the alkali solution is sodium hydroxide or ammonia water, and the mass concentration of sodium hydroxide is 200-400 g / L.

[0015] The application of the CO2 adsorption material prepared by the preparation method is as follows: for absorbing CO2 gas, controlling the concentration of CO2 gas to 10-99%, the flow rate of CO2 gas to 0.1-10L / min, the reaction time to 1-12 hours, and then desorbing to obtain a fixed carbon product.

[0016] The beneficial effects of the present invention after adopting the above technical solution are:

[0017] 1. The present invention uses steel slag, a large amount of difficult-to-treat solid waste generated in the production process of the steel industry, as raw material, and adopts a mixed flux melting-acid leaching-selective precipitation-drying-adsorption process, including mixing the steel slag with a flux, and then adding hydrochloric acid to dissolve the mixture. On the one hand, without changing its physical phase properties, the dissolution rate of the steel slag in the concentrated acid solution is accelerated by adding the flux, which helps the melting of the steel slag, making it easier to be chemically dissolved by hydrochloric acid and shortening the reaction time; on the other hand, hydrochloric acid is added to leach the steel slag to make it completely dissolved, and hydrochloric acid forms stable complex ions with many metal ions, making it an effective solvent for metal ores.

[0018] 2. The present invention adopts hydrofluoric acid solution as a selective leaching agent to strengthen the separation of calcium and silicon ions in steel slag, which helps to selectively leach silicon-containing ions from steel slag to generate volatile silicon tetrafluoride, thereby achieving the purpose of separation from calcium-containing compounds, thereby increasing the content of the final calcium-containing component compound and improving the carbon fixation efficiency of steel slag.

[0019] 3. The present invention improves the solubility of steel slag and the leaching rate of Ca element without adjusting the mineral composition of steel slag, and has a high carbon fixation efficiency. Compared with the existing steel slag CO2 fixation method, it has the advantages of short reaction time, high calcium oxide component conversion rate, and large amount of CO2 fixed per unit steel slag.

[0020] 4. The present invention adds alkali and selectively precipitates calcium ions, so that the Ca element is precipitated in the form of calcium hydroxide, thereby increasing the content of calcium hydroxide precipitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram of the process flow of a preparation method and application of a CO2 absorbing material modified and reconstructed by steel slag according to the present invention;

[0022] Figure 2 The phase composition spectrum of the adsorption material obtained in Examples 1 to 4;

[0023] Figure 3 To prepare the SEM image of the obtained CO2 adsorbent material, EDS spectrum analysis was performed on the marked B;

[0024] Figure 4 This is the EDS spectrum analysis diagram of point B in the SEM image of the prepared CO2 adsorption material. Figure 4 yes Figure 3 Surface scanning analysis result diagram at B in the middle;

[0025] Figure 5 It is the TG-DTG curve diagram in Example 1;

[0026] Figure 6 It is the TG-DTG curve diagram in Example 2;

[0027] Figure 7 It is the TG-DTG curve diagram in Example 3;

[0028] Figure 8 This is the TG-DTG curve diagram in Example 4. DETAILED DESCRIPTION

[0029] like Figure 1 As shown, a large amount of difficult-to-treat steel slag produced in the production process of the steel industry is selected. The steel slag contains a large amount of calcium-containing compounds and a small amount of free calcium oxide. The high content of calcium-containing compounds makes the steel slag an ideal raw material for mineral carbonation. The steel slag is converted into a stable carbonate by adsorbing CO2. The steel slag is first ball-milled, and then treated with mixed flux melting, acid leaching, adding alkali solution to selectively precipitate calcium ions, filtering, etc. Finally, the calcium oxide adsorption material is obtained after evaporating the water, which accelerates the acid dissolution rate of the steel slag and increases the content of calcium hydroxide precipitation. Specifically:

[0030] The raw steel slag and flux are mixed in a mass ratio of 1:1-20, and then reacted at a temperature of 800-1400°C for 5-120 minutes to completely melt the mixture, and then cooled into a solid state to obtain molten steel slag. The raw steel slag selected includes: converter steel slag or electric furnace steel slag, the particle size of the steel slag solid particles does not exceed 0.2mm, and the steel slag component content is required to be controlled within: CaO: 35%-50%, Fe2O3: 10%-30.5%, SiO2: 10%-20%, Al2O3: 0.5%-9%, MgO: 2%-10%, V2O5: 0.2%-8%, TiO2: 0.2%-0.9%, SrO: 0.01%-0.08%, CuO: 0.01%-0.08%, NbO: 0.02%-0.08%. The flux used is one or a combination of two of lithium tetraborate, lithium metaborate, sodium carbonate, boric acid, sodium peroxide, etc.

[0031] The obtained molten steel slag is crushed and ground into powder, the powder particle size does not exceed 0.2mm, and then hydrochloric acid with a concentration of 20% to 40wt% is added to completely dissolve it. The optimal concentration of hydrochloric acid is 30% to 37%. The solid-liquid ratio of the molten steel slag and the hydrochloric acid is 1:3 to 20g:ml. A leaching reaction occurs. During the leaching reaction, the reaction temperature is controlled at 90 to 400°C and the stirring speed is 30 to 180r / min. Then, hydrofluoric acid with a concentration of 20% to 50.0wt% is added to the dissolved solution, the mass of the hydrofluoric acid added is 1 to 2.6 times the mass of the steel slag, and the temperature is kept constant at 90 to 400°C for 20 to 180 minutes. After the reaction, perchloric acid with a concentration of 20% to 50.0wt% is added to the reaction solution, the mass of the perchloric acid added is 0.5 to 1.3 times the mass of the steel slag, and the solution is stirred at a constant temperature of 90 to 400°C at a speed of 30 to 180r / min for 20 to 180min. After stopping the stirring, the solution is cooled to room temperature to obtain a mixed solution.

[0032] Add alkali solution to the obtained mixed solution, adjust the pH value to 3-4 and 9-11, selectively adjust the solution pH through step-by-step precipitation, filter and separate Fe(OH)3 and Ca(OH)2, and precipitate iron and calcium ions step by step, that is, first adjust the solution pH to 3-4, filter after complete precipitation, continue to add alkali solution to the filtered filtrate to adjust the pH to about 9-11, filter and separate again after sufficient precipitation, and wash the filter residue obtained by the final filtration and separation with water for multiple times to obtain the initial adsorbent material. The number of water washings is ≥5 times, and the alkali solution is sodium hydroxide or ammonia water, wherein the mass concentration of sodium hydroxide is 200-400g / L.

[0033] The initial adsorbent material is kept at a temperature of 80 to 200° C. for 60 to 720 minutes to fully evaporate water vapor to prepare the desired high calcium-based CO2 adsorbent material, i.e., steel slag modified and reconstructed CO2 adsorbent material. The adsorbent material is white and flocculent ( Figure 3 As shown in the figure, the main components include: CaO: 56% ~ 75%, Fe2O3: 20% ~ 40%, SiO2: 0% ~ 13%, Al2O3: 0.07% ~ 0.5%, MgO: 1.2% ~ 1.4%, V2O5: 0.19% ~ 0.4%, SrO: 0.01% ~ 0.08%, MnO: 0.1% ~ 0.4%. It can be seen that it is mainly CaO and a small amount of Fe2O3, MgO, SiO2 and other phases, and is a highly efficient CO2 absorbent material.

[0034] The obtained CO2 adsorbent material absorbs CO2 gas, controls the concentration of CO2 gas to 10-99%, the flow rate of CO2 gas to 0.1-10L / min, and the reaction time to 1-12 hours, which can be carried out at room temperature and pressure or at room temperature and low pressure, and then desorbs to obtain a carbon fixation product. Figure 4 After the adsorption material absorbed CO2 gas, it was calculated that the carbon fixation efficiency reached 22.8~42.2kg / t. It can be seen that the amount of CO2 absorbed was large and the reaction speed was fast, indicating that the modified steel slag has good adsorption efficiency. Compared with the original steel slag directly absorbing CO2, the fixed amount per ton of steel slag is increased by about 8~39kg.

[0035] Four embodiments are provided below. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0036] Example 1

[0037] The steel slag particle size was crushed to less than 0.2 mm, 4 g of steel slag powder (composition includes: CaO: 45.7%, Fe2O3: 30.5%, SiO2: 12.9%, Al2O3: 1.06%, MgO: 5.2%, MnO: 3.7%, TiO2: 0.9%, SrO: 0.08%, CuO: 0.01%, NbO: 0.02%) was mixed evenly with 6 g of mixed reagent (lithium tetraborate: lithium metaborate = 67:33), and completely melted at 1400°C. After cooling to room temperature, a glassy phase steel slag sample was obtained, the sample was crushed and ground into powder, and then mixed with a hydrochloric acid solution with a mass concentration of 34% at a solid-liquid ratio of 1 g: 5.5 ml, and the mixture was continuously stirred for 3 hours at 90°C until the steel slag was completely dissolved. Then add 7 ml of hydrofluoric acid solution with a mass concentration of 40% to the mixed solution, keep the temperature at 90°C, add 5 ml of 40wt% perchloric acid solution after reacting for 40 minutes, and stir continuously for 20 minutes, then cool the mixed solution to room temperature. Then add sodium hydroxide solution to the obtained mixed solution, and adjust the solution pH to 3-4 to precipitate it. After the precipitation is complete, continue to add alkali to the filtrate to adjust the pH value to 10 after filtering, so that it is fully precipitated again, and filter again after the white precipitate is completely settled to obtain a clear liquid and a filter cake, rinse the filter cake five times with deionized water to obtain an undried initial adsorbent material, dry the obtained initial adsorbent material at 80°C for 12 hours, and then grind the sample evenly to use as a CO2 adsorbent material. After testing and analysis, it contains CaO: 46.1%, Fe2O3: 38.2%, SiO2: 12.9%, Al2O3: 0.5%, MgO: 1.3%, V2O5: 0.4%, SrO: 0.05%, MnO: 0.4%, and the phase structure is as follows Figure 2 The modified slag was placed in a closed device to adsorb CO2 gas at room temperature and pressure. The CO2 flow rate was set to 1L / min and the reaction was maintained for 3h. After the adsorption was completed, the material was subjected to thermogravimetric-differential thermal analysis, as shown in Figure 5 As shown in the figure, it is calculated that the carbon fixation efficiency of the modified steel slag is about 22.8kg / t.

[0038] Example 2

[0039] The steel slag particle size was crushed to less than 0.2 mm, 4 g of steel slag powder (composition includes: CaO: 35%, Fe2O3: 30.5%, SiO2: 10%, Al2O3: 9%, MgO: 2%, V2O5: 8%, TiO2: 0.2%, SrO: 0.01%, CuO: 0.08%, NbO: 0.08%) was taken and mixed evenly with 6 g of mixed reagent (lithium tetraborate: lithium metaborate = 67:33), and completely melted at 1000°C, and after cooling to room temperature, a glassy phase steel slag sample was obtained. The sample was crushed and ground into powder, and then mixed with a hydrochloric acid solution with a mass concentration of 20% at a solid-liquid ratio of 1 g: 3 ml, and the mixture was continuously stirred for half an hour at 240°C until the steel slag was completely dissolved. Then add 7ml of hydrofluoric acid solution with a mass concentration of 50% to the mixed solution, keep the temperature unchanged at 400°C, react for 20 minutes, add 5ml of 50.0wt% perchloric acid solution, and stir continuously for 180 minutes, then cool the mixed solution to room temperature. Then add sodium hydroxide solution to the obtained mixed solution, and adjust the solution pH to 3-4 to precipitate it. After precipitation is complete, continue to add alkali to the filtrate to adjust the pH to 9 after filtering, so that it is fully precipitated again, and filter again after the white precipitate is completely settled to obtain a clear liquid and a filter cake, rinse the filter cake five times with deionized water, place the obtained filter cake at 200°C and dry it for 1 hour, and then grind the dried sample evenly as a CO2 adsorbing material. After testing and analysis, it contains about CaO: 56%, Fe2O3: 20%, Al2O3: 0.07%, MgO: 1.4%, V2O5: 0.19%, SrO: 0.01%, MnO: 0.11%, and the phase structure is attached Figure 2 The modified slag was placed in a closed device to adsorb CO2 gas at room temperature and pressure. The CO2 flow rate was set to 0.1L / min and the reaction was maintained for 12h. After the adsorption was completed, the material was subjected to thermogravimetric-differential thermal analysis, as shown in Figure 6 As shown in the figure, it is calculated that the carbon fixation efficiency of the modified steel slag is about 25.1kg / t.

[0040] Example 3

[0041] The steel slag particle size was crushed to less than 0.2 mm, 8 g of steel slag powder (composition includes: CaO: 50%, Fe2O3: 10%, SiO2: 20%, Al2O3: 0.05%, MgO: 10%, V2O5: 0.2%, TiO2: 0.5%, SrO: 0.06%, CuO: 0.08%, NbO: 0.08%) was taken and mixed evenly with 24 g of mixed reagent (sodium carbonate: boric acid = 67:33), and completely melted at 800°C, and after cooling to room temperature, a glassy phase steel slag sample was obtained. The sample was crushed and ground into powder, and then mixed with a hydrochloric acid solution with a mass concentration of 40% at a solid-liquid ratio of 1 g: 7 ml, and the mixture was continuously stirred for 2 hours at 400°C until the steel slag was completely dissolved. Then add 15ml of hydrofluoric acid solution with a mass concentration of 20% to the mixed solution, keep the temperature unchanged at 400℃, react for 20 minutes, add 9ml of 20% perchloric acid solution, and stir continuously for 20 minutes, then cool the mixed solution to room temperature. Then add sodium hydroxide solution to the mixed solution, and adjust the solution pH to 3-4 to precipitate it. After precipitation is complete, filter and continue to add alkali to the filtrate to adjust the pH to 10, so that it is fully precipitated again. After the white precipitate is complete, filter again to obtain a clear liquid and a filter cake, rinse the filter cake five times with deionized water, place the obtained filter cake at 110℃ and dry it for 10 hours, and then grind the dried sample evenly as a CO2 adsorbing material. After testing and analysis, it contains CaO: 64.9%, Fe2O3: 32.8%, Al2O3: 0.07%, MgO: 1.2%, V2O5: 0.19%, SrO: 0.07%, MnO: 0.09%, and the phase structure is as shown in the attached Figure 2 The modified steel slag was placed in a closed device to adsorb CO2 gas at room temperature and pressure. The CO2 flow rate was set to 1L / min and the reaction was maintained for 3h. After the adsorption was completed, the material was subjected to thermogravimetric-differential thermal analysis, as shown in the attached figure. Figure 7 As shown in the figure, it is calculated that the carbon fixation efficiency of the modified steel slag is about 42.2kg / t.

[0042] Example 4

[0043] The steel slag was crushed to a particle size of less than 0.2 mm, 8 g of steel slag powder (components include: CaO: 45.7%, Fe2O3: 30.5%, SiO2: 12.9%, Al2O3: 1.06%, MgO: 5.2%, MnO: 3.7%, TiO2: 0.8%, SrO: 0.07%, CuO: 0.04%, NbO: 0.05%) was mixed evenly with 40 g (sodium carbonate: boric acid = 67:33) mixed reagent, and completely melted at high temperature. After cooling to room temperature, a glassy phase steel slag sample was obtained. The sample was crushed and ground into powder, and then mixed with a hydrochloric acid solution with a mass concentration of 37% at a solid-liquid ratio of 1 g: 7.5 ml, and the mixture was continuously stirred at 240°C for 3 hours until the steel slag was completely dissolved. A hydrofluoric acid solution with a mass concentration of 40% was added to the mixture. 20ml, keep the temperature unchanged at 240℃, after reacting for 40 minutes, add 11ml of 40% perchloric acid solution, and stir continuously for 10 minutes, then cool the mixture to room temperature. Then add sodium hydroxide solution to the mixed solution, and adjust the solution pH to 3-4 to make it precipitate. After the precipitation is complete, filter and continue to add alkali to the filtrate to adjust the pH to 10, so that it is fully precipitated again. After the white precipitate is complete, filter again to obtain a clear liquid and a filter cake. The obtained filter cake is placed at 110℃ and dried for 8 hours, and then the dried sample is ground evenly as a CO2 adsorption material. After detection and analysis, it contains CaO: 59.6%, Fe2O3: 38.5%, Al2O3: 0.08%, MgO: 1.2%, V2O5: 0.19%, SrO: 0.07%, MnO: 0.17%, and the phase structure is as follows Figure 2 The modified steel slag was placed in a closed device to adsorb CO2 gas at room temperature and pressure. The CO2 flow rate was set to 1L / min and the reaction was maintained for 3h. After the adsorption was completed, the material was subjected to thermogravimetric-differential thermal analysis, as shown in Figure 8 As shown in the figure, it is calculated that the carbon fixation efficiency of the modified steel slag is about 31kg / t.

Claims

1. A method for preparing a CO2 absorbing material by modifying and reconstructing steel slag, characterized in that The following steps are involved: Step 1): mixing the original steel slag with a flux, melting the mixture at a temperature of 800 to 1400° C., and cooling the mixture to obtain molten steel slag; Step 2): adding hydrochloric acid to the molten slag to completely dissolve it to obtain a solution, adding hydrofluoric acid to the solution, reacting at a temperature of 90 to 400° C. to obtain a reaction solution, then adding perchloric acid to the reaction solution, stirring at a constant temperature of 90 to 400° C., stopping stirring and cooling to room temperature to obtain a mixed solution; Step 3): adding alkali solution to the mixed solution to selectively adjust the pH value to 3-4 and 9-11, selectively precipitating step by step, so that iron and calcium ions are precipitated step by step to obtain filter residues, and washing the filter residues to obtain initial adsorptive materials; Step 4): The initial adsorbent material is fully evaporated to produce the desired CO2 adsorbent material.

2. The preparation method according to claim 1, characterized in that: In step 1), the flux is one or a combination of lithium tetraborate, lithium metaborate, sodium carbonate, boric acid, and sodium peroxide, the mass ratio of the original steel slag to the flux is 1:1-20, and the melting time is 5-120 minutes.

3. The preparation method according to claim 1, characterized in that: In step 1), the original slag includes: converter slag or electric furnace slag, the particle size of the solid particles of the slag does not exceed 0.2 mm, and the composition content of the slag is required to be controlled within the following ranges: CaO: 35% to 50%, Fe2O3: 10% to 30.5%, SiO2: 10% to 20%, Al2O3: 0.5% to 9%, MgO: 2% to 10%, V2O5: 0.2% to 8%, TiO2: 0.2% to 0.9%, SrO: 0.01% to 0.08%, CuO: 0.01% to 0.08%, and NbO: 0.02% to 0.08%.

4. The preparation method according to claim 1, characterized in that: In step 2), the molten steel slag is first ground into powder with a particle size not exceeding 0.2 mm, and then hydrochloric acid with a concentration of 20% to 40wt% is added.

5. The preparation method according to claim 1, characterized in that: In step 2), The solid-liquid ratio of the molten steel slag to the hydrochloric acid is 1:3-20; The concentration of the hydrofluoric acid is 20% to 50.0 wt%, and the mass of the added hydrofluoric acid is 1 to 2.6 times the mass of the original slag; The concentration of the perchloric acid is 20% to 50.0 wt%, and the mass of the added perchloric acid is 0.5 to 1.3 times the mass of the original slag; The stirring speed is 30-180 r / min, and the stirring time is 20-180 min.

6. The preparation method according to claim 1, characterized in that: In step 3), the alkali solution is sodium hydroxide or ammonia water, and the mass concentration of sodium hydroxide is 200-400g / L.

7. The preparation method according to claim 5, characterized in that: In step 3), the number of water washings is ≥5 times.

8. The preparation method according to claim 1, characterized in that: In step 4), the initial adsorbent material is kept at a temperature of 80 to 200° C. for 60 to 720 minutes to fully evaporate the water vapor.

9. An application of a CO2 adsorbent material prepared by the preparation method according to claim 1, characterized in that: Used for Absorb CO2 gas, control the concentration of CO2 gas to 10-99%, the flow rate of CO2 gas to 0.1-10L / min, the reaction time to 1-12 hours, and then desorb to obtain a fixed carbon product.

10. The use according to claim 9, characterized in that: Absorb CO2 gas at normal temperature and pressure or at normal temperature and low pressure.

Citation Information

Patent Citations

  • Method for preparing calcium oxide based CO2 cyclic adsorbing material from steel slag

    CN103801253A

  • Method for preparing calcium-based cyclic carbon capture material from steel slag

    CN114832770A

  • Method for enriching and recovering calcium and iron through steel slag melting-wet separation

    CN117025862A

  • Method for preparing nano calcium carbonate through carbon dioxide adsorption by using steel slag

    CN117185334A

  • Method for preparing CO2 adsorbent from converter slag and use method of adsorbent

    CN117839620A

Cited By

  • Preparation method of ultrahigh-adsorption-rate steel slag-based carbon dioxide adsorption material