Magnesium iron oxide / magnetite core-shell nano material, preparation method and application thereof, and phosphorus removal adsorbent
The core-shell structure nanomaterial formed by mafen oxide coated with magnetite solves the problem that the adsorption shell is prone to fall off during the recycling process of magnetite core-shell materials, and improves the adsorption performance and material stability of phosphate. Efficient phosphate recycling and multiple recycling are achieved.
Patent Information
- Application Number
- CN202411053462.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
During the recycling process, the adsorption shell of the existing magnetite core-shell nanomaterials are easily separated from the magnetite surface, resulting in reduced performance and potential health risks. The existing phosphorus removal process produces a large amount of waste sludge, making it difficult to efficiently recover phosphate.
Using the preparation method of mafite oxide/magnetite core-shell structure nanomaterials, a stable Mafice oxide coats the magnetite core-shell structure, weakens magnetite growth, increases particle size, and improves stability and adsorption performance.
It significantly improves the stability and reusability of mafite oxide/magnetite core-shell structure nanomaterials, enhances the adsorption capacity to phosphate, and the saturation adsorption amount at room temperature is as high as 90.2~100.8 mg P/g, and in many cases The phosphorus adsorption amount of more than 80% was maintained during the cycle, and the magnesium loss rate was reduced.
Smart Images

Figure CN118976459A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental pollution remediation, and in particular to a magnesium iron oxide / magnetite core-shell nano material, and a preparation method, application, and phosphorus removal adsorbent thereof. Background Art
[0002] Core-shell nanoparticles have attracted increasing attention due to their high surface area, high activity, and controllable surface modification. Reusable core-shell nanoparticles can improve the economic feasibility of materials, and magnetic core-shell nanocomposites have attracted much interest due to the effect of allowing rapid separation from water using an external magnetic field. Available magnetic cores include metals (Fe, Co), metal alloys (Pd, Ni), and iron oxides (Fe3O4, CoFe2O4). Among them, magnetite has attracted great interest due to its rich oxygen content, low cost, and ability to facilitate rapid and low-energy magnetic separation recovery. To date, a variety of functional shells have been developed through various synthesis methods of magnetite core-shell nanoparticles, including oxides (MnO2 and ZnO), aluminosilicates (zeolites), and precious metals (Pt, Au), thereby expanding the application of magnetite core / shell nanocomposites. However, these strategies have some technical drawbacks in practical applications, mainly due to the weak interaction between the core and the shell, which leads to the easy separation of the active shell from the magnetite surface. This loss of nanoshells leads to performance degradation and poses potential health risks to the ecosystem.
[0003] Phosphorus resources have gradually become one of the biggest issues facing global sustainability in the 21st century. At the same time, a large amount of phosphorus is released from industry and agriculture into water bodies, causing serious eutrophication. The above problems highlight the necessity of efficient phosphate removal and recycling of nutrient wastewater with high phosphate content. Existing studies have explored and implemented various phosphorus removal processes, such as precipitation and activated sludge, but the large amount of waste sludge produced makes the extraction of phosphorus extremely difficult. In recent years, there have been many studies on magnetite core-shell nanoparticles for wastewater phosphate recovery, such as Fe3O4@MgAl-LDH@La(OH)3 coated with double metal hydroxides.
[0004] However, in the process of realizing the present invention, the applicant found that the problem of the adsorption shell falling off from the magnetite surface during the recovery process has not been solved, and there is an urgent need to develop a stable and recyclable metal oxide / magnetite core-shell nanoparticle for adsorbing phosphate. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of this, the present invention specifically provides a magnesia iron oxide / magnetite core-shell structure nanomaterial, and its preparation method, application, and phosphorus removal adsorbent, in the hope of improving the stability and reusability of the magnetic core-shell material, and improving the phosphate recovery performance of the magnetic core-shell material.
[0007] (II) Technical solution
[0008] According to a first aspect of the present invention, a method for preparing a ferrous oxide / magnetite core-shell structure nanomaterial is provided. The method for preparing a ferrous oxide / magnetite core-shell structure nanomaterial comprises:
[0009] Adding magnesium salt and ferrous salt to an acidic solution to form solution A;
[0010] providing an alkaline solution containing an oxidant to form a solution B;
[0011] Mix solution A and solution B to form solution C;
[0012] Solution C is subjected to a hydrothermal chemical reaction to obtain a magnesium iron oxide / magnetite core-shell structure nanomaterial.
[0013] In some embodiments of the present invention, in the step of adding magnesium salt and ferrous salt to the acidic solution, the magnesium salt is one of the following materials: magnesium chloride, magnesium sulfate, and magnesium nitrate.
[0014] In some embodiments of the present invention, the ferrous salt is one of the following materials: ferrous sulfate, ferrous chloride.
[0015] In some embodiments of the present invention, the acidic solution is a hydrochloric acid solution containing a reducing agent, the pH of the solution is lower than 1.0, and the reducing agent is one or more of the following materials: hydrazine hydrate, ascorbic acid, sodium borohydride.
[0016] In some embodiments of the present invention, in the step of providing an alkaline solution containing an oxidant, the oxidant is sodium nitrate.
[0017] In some embodiments of the present invention, the alkaline solution is a solution of the following materials: sodium hydroxide or potassium hydroxide.
[0018] In some embodiments of the present invention, the magnesium salt is magnesium chloride; the ferrous sulfate is ferrous sulfate heptahydrate; the acidic solution is a hydrochloric acid solution containing a reducing agent, the solution pH is lower than 1.0, and the reducing agent is ascorbic acid; the oxidant is sodium nitrate; and the alkaline solution is a sodium hydroxide solution.
[0019] In some embodiments of the present invention, the molar ratio of magnesium chloride to ferrous sulfate heptahydrate is between 1:39 and 1:4.
[0020] In some embodiments of the present invention, in solution A, the total molar concentration of magnesium ions and ferrous ions is between 0.01 and 0.15 mol / L.
[0021] In some embodiments of the present invention, the mass concentration of ascorbic acid in the hydrochloric acid solution containing the reducing agent is 0.5-2.0 g / .
[0022] In some embodiments of the present invention, in solution B, the concentration of sodium hydroxide is 2.5-5 mol / L, and the concentration of sodium nitrate is 0.6-1.2 mol / L.
[0023] In some embodiments of the present invention, the step of mixing solution A and solution B comprises: dropping solution A into solution B; or dropping solution B into solution A at a rate of 2 to 5 ml / min.
[0024] In some embodiments of the present invention, the step of subjecting solution C to a hydrothermal chemical reaction comprises: heating solution C in a water bath to 80-95° C. to subject the solution to a hydrothermal chemical reaction.
[0025] In some embodiments of the present invention, before the step of mixing solution A and solution B, the step further includes: purging solution A and solution B with nitrogen for 30 minutes each; and / or heating solution B in a water bath to 80-95° C.
[0026] In some embodiments of the present invention, in the step of heating solution C to 80-95° C. in a water bath for a hydrothermal chemical reaction: the hydrothermal chemical reaction is carried out in a conical flask; and / or, nitrogen is purged during the hydrothermal chemical reaction; and / or, the magnetic stirring rate is maintained at 250-500 rpm for 3-6 hours.
[0027] According to a second aspect of the present invention, a magnesium iron oxide / magnetite core-shell structure nanomaterial is provided. The magnesium iron oxide / magnetite core-shell structure nanomaterial is obtained by the above preparation method.
[0028] According to a third aspect of the present invention, there is provided an application of the above-mentioned magnesium iron oxide / magnetite core-shell structure nanomaterial for removing phosphate ions in water environment remediation.
[0029] According to a fourth aspect of the present invention, a dephosphorization adsorbent is provided, which comprises: the above-mentioned magnesium iron oxide / magnetite core-shell structure nanomaterial.
[0030] (III) Beneficial effects
[0031] It can be seen from the above technical solution that the present invention has at least one of the following beneficial effects compared with the prior art:
[0032] (1) In the present invention, magnesium iron oxide is used to coat magnetite to form a core-shell nanomaterial, which weakens the agglomeration effect of the magnetite material, relatively increases the specific surface area, and improves the van der Waals force, which is beneficial to the removal of phosphate ions in polluted water.
[0033] (2) The applicant has proved through experiments that the particle size of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared using iron salt and ferrous salt is significantly increased. Furthermore, due to the large particle size, the core-shell structure is unstable and the adsorption shell is easily detached from the magnetite surface.
[0034] During the preparation process of the present invention, only ferrous salts are added instead of ferric salts and ferrous salts. At the same time, reducing agents such as ascorbic acid are added to the solution, N2 is purged before and after the reaction process, and the temperature of the solution is controlled, thereby weakening the growth of magnetite during the oxidation process, making the radius of magnetite particles coated with magnesium ferrite relatively reduced, making the core-shell structure more stable, and greatly reducing the proportion of adsorption shell shedding, which is conducive to the continuous release of the phosphate removal effect.
[0035] (3) Experiments have confirmed that the magnesium iron oxide / magnetite core-shell structure nanomaterial of the present invention has a high adsorption capacity for phosphate pollutants. At room temperature, its saturated adsorption capacity for phosphorus is as high as 90.2-100.8 mg P / g. In addition, after 8 desorption-adsorption cycles, the phosphorus adsorption capacity remains above 80% while the magnesium loss rate is less than 12%. In contrast, the magnesium loss rate of the magnesium hydroxide-coated magnetite core-shell structure nanomaterial reaches above 95%. Therefore, the magnesium iron oxide / magnetite core-shell structure nanomaterial of the present invention is an excellent phosphate adsorbent and has good reusability.
[0036] (4) In the present invention, the magnesium iron oxide / magnetite core-shell structure nanomaterial has excellent material stability. Experiments have shown that under the condition of pH 3-8, Mg 2+ The release concentration of magnesium hydroxide / magnetite core-shell nanomaterials is 1-2.3 μg / L, which is lower than the acceptable range of natural aquatic environment (i.e. element Mg < 2.3 μg / L). 2+ The concentration is 10~23.6μg / L. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The present invention is a flow chart of the method for preparing the magnesium iron oxide / magnetite core-shell structure nanomaterial.
[0038] Figure 2 This is the X-ray diffraction pattern of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared in Example 1.
[0039] Figure 3These are the transmission electron microscope images and energy dispersive X-ray surface scan and line scan images of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared in Example 1 after focused ion beam sectioning.
[0040] Figure 4 This is the phosphorus absorption curve of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared in Example 1 under different phosphate concentration conditions.
[0041] Figure 5 It is a comparison chart of magnesium loss rate of magnesium iron oxide / magnetite core-shell structure nanomaterial and magnesium hydroxide / magnetite core-shell structure nanomaterial prepared by the method of Example 3 in 8 adsorption-desorption cycles.
[0042] Figure 6 This is a graph showing the change in phosphorus adsorption during each adsorption-desorption cycle of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared by the method of Example 3. DETAILED DESCRIPTION
[0043] The purpose of the present invention is to provide a magnesium iron oxide / magnetite core-shell structure nanomaterial in view of the shortcomings of the above-mentioned existing magnetic core-shell materials in actual use, so as to improve the stability of the core-shell structure, thereby improving the phosphorus adsorption capacity and economic benefits of the magnetic core-shell material in water environment remediation applications.
[0044] The present invention firstly provides a method for preparing a magnesium iron oxide / magnetite core-shell structure nano material. Figure 1 This is a flow chart of the preparation method of the magnesium iron oxide / magnetite core-shell structure nanomaterial of the present invention. Please refer to Figure 1 The preparation method of the magnesium iron oxide / magnetite core-shell structure nanomaterial of the present invention comprises:
[0045] Step S1, adding magnesium salt and ferrous salt to an acidic solution to form solution A;
[0046] Step S2, providing an alkaline solution containing an oxidant to form a solution B;
[0047] Step S3, mixing solution A and solution B to form solution C;
[0048] Step S4, performing a hydrothermal chemical reaction on the solution C to obtain a magnesium iron oxide / magnetite core-shell structure nanomaterial.
[0049] In a preferred embodiment of the present invention, in step S1, the magnesium salt is magnesium chloride; the ferrous salt is ferrous sulfate, more specifically ferrous sulfate heptahydrate, the molar ratio of magnesium chloride to ferrous sulfate heptahydrate is between 1:39 and 1:4, and the pH of the hydrochloric acid solution is less than 1.0. Moreover, in solution A, the total molar concentration of magnesium ions and ferrous ions is between 0.01 and 0.15 mol / L. In addition, the hydrochloric acid solution is an acidic solution containing ascorbic acid, wherein the mass concentration of ascorbic acid is 0.5 to 2.0 g / L.
[0050] Those skilled in the art will appreciate that, in addition to magnesium chloride, other magnesium salts with similar properties may also be used, such as magnesium sulfate and magnesium nitrate. Similarly, in addition to ferrous sulfate, other ferrous salts with similar properties may also be used, such as ferrous chloride. These variations and equivalents that those skilled in the art can think of may also implement the present invention, and are also within the scope of protection of the present invention.
[0051] It should be particularly noted that the present invention only adds ferrous salts instead of adding ferric salts and ferrous salts at the same time, and ascorbic acid is added to solution A and N2 is purged to avoid premature oxidation of divalent iron to trivalent iron. This is to weaken the growth of magnetite during the oxidation process and relatively reduce the radius of the magnetite particles coated with magnesium ferrite.
[0052] It will be appreciated by those skilled in the art that ascorbic acid is used as a reducing agent during the preparation process to prevent ferrous iron from being oxidized to ferric iron. The ascorbic acid can also be replaced by reducing agents such as hydrazine hydrate and sodium borohydride. Purging solution A with N2 before the hydrothermal reaction is also to prevent ferrous iron from being oxidized to ferric iron.
[0053] In a preferred embodiment of the present invention, in step S2, solution B is: sodium hydroxide or potassium hydroxide mixed with sodium nitrate solution. Specifically, solution B is a mixture of sodium hydroxide and sodium nitrate, the concentration of sodium hydroxide is 2.5-5 mol / L, and the concentration of sodium nitrate is 0.6-1.2 mol / L.
[0054] In a preferred embodiment of the present invention, step S3 comprises: adding solution A dropwise to solution B. Before the addition, nitrogen is purged for 30 minutes each for solution A and solution B, solution B is heated to 80-95° C. in a water bath, and then solution B is added dropwise to solution A at a rate of 2-5 ml / min to form solution C.
[0055] In a preferred embodiment of the present invention, step S4 comprises: in the step of subjecting solution C to a hydrothermal chemical reaction, the hydrothermal chemical reaction is carried out in a conical flask, the solution C is kept in a water bath at 80-95° C., the magnetic stirring rate is maintained at 250-500 rpm, and the temperature is maintained for 3-6 hours, and nitrogen purge is maintained.
[0056] It should be noted that the present invention adopts a high-temperature hydrothermal reaction at 90° C. and controls the ratio of magnesium to iron to prepare an impurity-free magnesium-iron oxide / magnetite core-shell structure nanomaterial.
[0057] Based on the above preparation method, the present invention provides an impurity-free magnesium iron oxide / magnetite core-shell structure nanomaterial obtained by the preparation method.
[0058] Based on the above-mentioned magnesium iron oxide / magnetite core-shell structure nanomaterial, the present invention also provides an application of the magnesium iron oxide / magnetite core-shell structure nanomaterial in adsorbing phosphate in a water environment.
[0059] Based on the above-mentioned magnesium iron oxide / magnetite core-shell structure nanomaterial, the present invention also provides a dephosphorus adsorbent. The dephosphorus adsorbent comprises: the above-mentioned magnesium iron oxide / magnetite core-shell structure nanomaterial.
[0060] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.
[0061] Example 1
[0062] (1) Magnesium chloride and ferrous sulfate heptahydrate were added to 100 ml of hydrochloric acid solution containing 0.1 g of ascorbic acid (pH < 1.0) to form solution A, which was purged with N2 for 30 min. The total metal concentration in solution A was 0.09 mol / L.
[0063] (2) Sodium hydroxide and sodium nitrate were added into 100 ml of deionized water to form solution B, wherein the concentration of sodium hydroxide was 4 mol / L and the concentration of sodium nitrate was 0.9 mol / L.
[0064] (3) Solution B was added to a conical flask, heated in a water bath to 80-95°C, and purged with N2 for 30 min. Solution A was then added to solution B at a rate of 4 ml / min to obtain solution C.
[0065] (4) maintaining solution C in a water bath at 90° C., maintaining a magnetic stirring rate of 300 rpm for 4 h, and maintaining nitrogen purge to obtain a magnesium iron oxide / magnetite core-shell structured nanomaterial.
[0066] The structure of the obtained MgFeO2 / magnetite core-shell structured nanomaterials was determined by X-ray diffraction (XRD). Figure 2 This is the X-ray diffraction pattern of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared in Example 1. Figure 2 In the figure, the upper figure is the X-ray diffraction spectrum of the sample in this embodiment; the lower figure is the standard diffraction peak of magnetite. Figure 2It can be seen that the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared in this example has characteristic diffraction peaks belonging to magnetite.
[0067] Example 1 Preparation of the sample after focused ion beam sectioning (FIB) transmission electron microscope (TEM) image and energy dispersive X-ray (EDS) surface scan and line scan images are as follows Figure 3 shown. Specifically, Figure 3 In the figure, (a) is a TEM image of the sample of Example 1; (b) is a high-resolution TEM image of the sample of Example 1, wherein Core represents "core" and Shell represents "shell"; (c) is an EDS surface scan image of the sample of Example 1, and the elements include iron, magnesium and oxygen; (d) is an EDS line scan image shown in (a), and the elements include iron, magnesium and oxygen. Figure 3 It can be seen from the figures that the MgFeO2 / magnetite core-shell structure nanomaterials are obvious spherical shell structures.
[0068] The test shows that the phosphorus adsorption capacity of the magnesium iron oxide / magnetite core-shell structure nanomaterial can be tested using a sequencing batch adsorption experiment. Figure 4 This is the phosphorus absorption curve of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared in Example 1 under different phosphate concentration conditions. Figure 4 As shown, the adsorption capacity of phosphate by the magnesium iron oxide / magnetite core-shell structured nanomaterial is 95.8 mg P / g.
[0069] Example 2
[0070] (1) Magnesium chloride and ferrous sulfate heptahydrate were added to 100 ml of hydrochloric acid solution containing 0.5 g of ascorbic acid (pH < 1.0) to form solution A, which was purged with N2 for 30 min. The total metal concentration in solution A was 0.045 mol / L.
[0071] (2) Sodium hydroxide and sodium nitrate were added into 100 ml of deionized water to form solution B, wherein the concentration of sodium hydroxide was 2.5 mol / L and the concentration of sodium nitrate was 0.6 mol / L.
[0072] (3) Solution B was added to a conical flask, heated to 80°C in a water bath, and purged with N2 for 30 min. Solution A was then added to solution B at a rate of 5 ml / min to obtain solution C.
[0073] (4) maintaining solution C in a water bath at 80° C., maintaining a magnetic stirring rate of 250 rpm for 3 h, and maintaining nitrogen purge to obtain a magnesium iron oxide / magnetite core-shell structured nanomaterial.
[0074] The test shows that the phosphorus adsorption capacity of the magnesium iron oxide / magnetite core-shell structure nanomaterial is tested by batch adsorption experiment, and its adsorption amount of phosphate is 90.2 mg·P / g·adsorbent.
[0075] Example 3
[0076] (1) Magnesium chloride and ferrous sulfate heptahydrate were added to 100 ml of hydrochloric acid solution (pH < 1.0) containing 0.2 g of ascorbic acid to form solution A, which was purged with N2 for 30 min. The total metal concentration in solution A was 0.15 mol / L.
[0077] (2) Add sodium hydroxide and sodium nitrate to 100 ml of deionized water to form solution B. The concentration of sodium hydroxide is 5 mol / L and the concentration of sodium nitrate is 1.2 mol / L.
[0078] (3) Solution B was added to a conical flask, heated to 95°C in a water bath, and purged with N2 for 30 min. Solution A was then added to solution B at a rate of 2.5 ml / min to obtain solution C.
[0079] (4) maintaining solution C in a water bath at 95° C., maintaining a magnetic stirring rate of 500 rpm for 6 h, and maintaining nitrogen purge to obtain a magnesium iron oxide / magnetite core-shell structured nanomaterial.
[0080] The test shows that the phosphorus adsorption capacity of the magnesium iron oxide / magnetite core-shell structure nanomaterial was tested by batch adsorption experiments, and its adsorption capacity of phosphate was 100.8 mg P / g.
[0081] Furthermore, 8 adsorption-desorption cycles were used to compare the reusability of the magnesium iron oxide / magnetite core-shell structure nanomaterials prepared by the method of Example 3. Figure 5 The figure is a comparison of the magnesium loss rate of the magnesium iron oxide / magnetite core-shell structure nanomaterial and the magnesium hydroxide / magnetite core-shell structure nanomaterial prepared by the method of Example 3 in 8 adsorption-desorption cycles. Figure 5 As shown, the magnesium loss rate of the ferrous oxide / magnetite core-shell structure nanomaterial prepared by the method of Example 3 is less than 12%, while the magnesium loss rate of the magnesium hydroxide / magnetite core-shell structure nanomaterial is as high as over 95%. Figure 6 The graph is a graph showing the change in phosphorus adsorption during each adsorption-desorption cycle of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared by the method of Example 3. Figure 6 As shown, the phosphorus adsorption capacity of the magnesium iron oxide / magnetite core-shell structure nanomaterial prepared by the method of Example 3 is still maintained above 85% after multiple cycles, and the phosphorus desorption efficiency is also above 80%.
[0082] So far, the various embodiments of the present invention have been introduced.
[0083] In summary, the present invention provides a preparation method for a core-shell structure material formed by coating magnetite with magnesium iron oxide, so that the particle size of the magnetite-based material is reduced and the specific surface area is relatively increased. In the preparation method, only ferrous salts are added instead of iron salts and ferrous salts in order to weaken the growth of magnetite during the oxidation process. At the same time, the addition of a reducing agent, N2 purging before and after the reaction process, and the temperature control of the solution are used to avoid it as much as possible. In the above manner, the radius of the magnetite particles coated with magnesium iron oxide is relatively reduced, and the stability of the core-shell structure is enhanced. Experiments have shown that the magnesium iron oxide / magnetite core-shell structure nanomaterial of the present invention not only maintains the excellent magnetic selectivity of magnetite, but also avoids Mg after multiple regeneration cycles. 2+ A large amount of loss is avoided, thus ensuring that the material can still have high phosphorus adsorption and desorption efficiency after multiple recycling, so it has good application prospects.
[0084] It should be noted that some embodiments are not key elements of the present invention, but are known to those skilled in the art. They are not described in detail in the drawings or the body of the specification. In this case, they can be understood by referring to the relevant prior art. The above section has described the embodiments of the present invention in as much detail as possible in combination with the drawings. Based on the above description, those skilled in the art should have a clear understanding of the present invention.
[0085] Unless otherwise expressly stated in the description of the invention, the numerical parameters given in the description of the invention and the claims of the invention may be approximate and may vary according to the content of the invention. Specifically, all numerical values indicating the content of ingredients, reaction conditions, etc. recorded in the description and claims are understood to be modified by "about" in any case, which means that they include changes of ±10% in some embodiments, ±5% in some embodiments, ±1% in some embodiments, and ±0.5% in some embodiments. In addition, the word "comprising" does not exclude the existence of steps not listed in the requirements.
[0086] The Arabic numerals used in the specification and claims to indicate ordinal numbers are intended to modify the corresponding steps. Their original intention is only to clearly distinguish a step with a certain name from another step with the same name. It does not mean that a certain step has any ordinal number, nor does it mean the sequential relationship between one step and another step.
[0087] Likewise, it should be understood that in order to simplify the present invention and facilitate understanding of various aspects of the invention, in the above description of exemplary embodiments of the present invention, various features of the present invention are sometimes grouped into one embodiment, figure or description. However, the method of the invention should not be interpreted as reflecting the intention that the claimed invention requires more features than those explicitly stated in each claim. Specifically, as reflected in the claims, each creative aspect includes fewer features than all the features of the previous embodiments. In addition, based on design and reliability considerations, the embodiments can be used interchangeably or mixed with other embodiments, that is, the technical features of different embodiments can be freely combined to form more embodiments. Therefore, the claims following a specific embodiment are explicitly included in the specific embodiment, and each claim is regarded as a separate embodiment of the present invention.
[0088] Similarly, it should be understood that in order to simplify the present invention and help understand one or more of the various inventive aspects, in the above description of the exemplary embodiments of the present invention, the various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, as explained in the claims, the various aspects of the present invention are less than all the features of the aforementioned single embodiment. In addition, for design and reliability considerations, the embodiments can be mixed and matched with each other or with other embodiments, that is, the technical features of different embodiments can be freely combined to form complementary embodiments. Therefore, the claims following a specific embodiment are explicitly included in the specific embodiment, and each claim is regarded as a separate embodiment of the present invention.
[0089] The specific embodiments listed above provide a detailed description of the purpose, technical means and gain effects of the present invention. It should be understood that the detailed description is to enable those skilled in the art to better understand the present invention, rather than to limit the present invention, and all modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing a magnesium iron oxide / magnetite core-shell structure nanomaterial, It is characterized in that include: Adding magnesium salt and ferrous salt to an acidic solution to form solution A; providing an alkaline solution containing an oxidant to form a solution B; Mix solution A and solution B to form solution C; Solution C is subjected to a hydrothermal chemical reaction to obtain a magnesium iron oxide / magnetite core-shell structure nanomaterial.
2. The preparation method according to claim 1, It is characterized in that In the step of adding magnesium salt and ferrous salt to the acidic solution, The magnesium salt is one of the following materials: magnesium chloride, magnesium sulfate, magnesium nitrate; And / or, the ferrous salt is one of the following materials: ferrous sulfate, ferrous chloride; And / or, the acidic solution is a hydrochloric acid solution containing a reducing agent, the pH of the solution is lower than 1.0, and the reducing agent is one or more of the following materials: hydrazine hydrate, ascorbic acid, sodium borohydride.
3. The preparation method according to claim 2, It is characterized in that In the step of providing an alkaline solution containing an oxidant, The oxidant is sodium nitrate; And / or, the alkaline solution is a solution of the following materials: sodium hydroxide or potassium hydroxide.
4. The preparation method according to claim 3, It is characterized in that The magnesium salt is magnesium chloride; The ferrous sulfate is: ferrous sulfate heptahydrate; The acidic solution is a hydrochloric acid solution containing a reducing agent, the pH of the solution is lower than 1.0, and the reducing agent is: ascorbic acid; The oxidant is sodium nitrate; The alkaline solution is a sodium hydroxide solution.
5. The preparation method according to claim 4, It is characterized in that The molar ratio of magnesium chloride to ferrous sulfate heptahydrate is between 1:39 and 1:4; and / or, in solution A, the total molar concentration of magnesium ions and ferrous ions is between 0.01 and 0.15 mol / L; and / or, in the hydrochloric acid solution containing the reducing agent, the mass concentration of ascorbic acid is 0.5 to 2.0 g / L; And / or, in solution B, the concentration of sodium hydroxide is 2.5-5 mol / L, and the concentration of sodium nitrate is 0.6-1.2 mol / L.
6. The preparation method according to claim 1, It is characterized in that The step of mixing solution A and solution B comprises: dropping solution A into solution B; or dropping solution B into solution A at a rate of 2 to 5 ml / min; And / or, the step of performing a hydrothermal chemical reaction on the solution C includes: heating the solution C in a water bath to 80-95° C. to perform a hydrothermal chemical reaction.
7. The preparation method according to claim 6, It is characterized in that Before the step of mixing solution A and solution B, the step further includes: purging solution A and solution B with nitrogen for 30 minutes each; and / or, heating solution B in a water bath to 80-95° C.; And / or, in the step of heating solution C to 80-95° C. in a water bath for hydrothermal chemical reaction: the hydrothermal chemical reaction is carried out in a conical flask; and / or, nitrogen is purged during the hydrothermal chemical reaction; and / or, the magnetic stirring rate is maintained at 250-500 rpm for 3-6 hours.
8. A magnesium iron oxide / magnetite core-shell structure nanomaterial, It is characterized in that Obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the magnesium iron oxide / magnetite core-shell structure nanomaterial as claimed in claim 8 in the adsorption of phosphate ions for water environment restoration.
10. A phosphorus removal adsorbent, It is characterized in that include: The magnesium iron oxide / magnetite core-shell structure nanomaterial as described in claim 8.
Citation Information
Patent Citations
Lanthanum-based isomorphic replacement magnetite material, preparation method and application thereof, and phosphorus removal agent
CN116116369A
Modified magnesium-iron layered double-metal hydroxide adsorbent as well as preparation and application thereof
CN116920803A
Composite adsorbent and preparation method thereof
CN117123183A