Preparation method of low-palladium-content high-selectivity palladium catalyst for fixed bed anthraquinone hydrogenation
By preparing a high-selective palladium catalyst with a large pore size mesoporous structure, the problems of unstable catalyst hydrogenation and many by-products in the fixed bed device are solved, and high selectivity and low cost in extreme operating conditions are achieved Production, suitable for industrial applications.
Patent Information
- Application Number
- CN202411054406.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing fixed bed hydrogen peroxide device, the uneven distribution of working fluid caused by catalyst loading problems or flow fluctuations leads to unstable catalyst hydrogenation, resulting in harmful degradation substances, increasing the cost of anthraquinone and regenerated alumina, and in extreme labor Insufficient performance in the case.
The preparation method of low palladium content and high selectivity palladium catalyst is adopted. By mixing aluminum raw materials evenly with acid solution, forming colloids, and then adding a curing agent to form. After aging, washing, drying and calcining, alumina ball carrier is prepared and passed Ultrasonic treatment and negative pressure spraying of palladium liquid control the distribution of palladium on the surface of the support to form a palladium catalyst with a large pore mesoporous structure.
Under normal and high temperature conditions, the selectivity of palladium catalysts has been significantly improved, reducing by-products, reducing the impact of excessive hydrogenation and temperature deviation, reducing costs, and suitable for large-scale industrial production.
Smart Images

Figure CN118976484A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a palladium catalyst, in particular to a method for preparing a palladium catalyst with low palladium content and high selectivity for fixed-bed anthraquinone hydrogenation, and belongs to the technical field of palladium catalyst preparation methods. Background Art
[0002] At present, the main method for producing hydrogen peroxide worldwide is the anthraquinone method. The anthraquinone method refers to the catalytic hydrogenation of alkyl anthraquinone in a solvent to generate hydroanthraquinone, and then the hydroanthraquinone is oxidized by air to generate alkyl anthraquinone and hydrogen peroxide. The generated hydrogen peroxide is extracted with deionized water and collected, and the raffinate is recycled after regeneration. The existing anthraquinone method for producing H2O2 is generally divided into two methods: fluidized bed and fixed bed. At present, domestic H2O2 production companies generally use fixed beds, and their working fluids are composed of: 2-ethylanthraquinone (2-EAQ), tetrahydro-2-ethylanthraquinone (4H-2-EAQ), heavy aromatics, trioctyl phosphate, TBU, etc. In general, the anthraquinone method mainly includes four processes: hydrogenation, oxidation, extraction and post-treatment. Among them, catalytic hydrogenation is the key step in the production of hydrogen peroxide by the anthraquinone method. Highly active and highly selective catalysts can effectively improve the hydrogenation efficiency and reduce the degradation of anthraquinone.
[0003] At present, fixed-bed hydrogen peroxide plants account for the majority in my country. During the production process, due to various reasons such as catalyst loading problems or flow fluctuations, the working fluid is unevenly distributed, resulting in biased flow, which makes the catalyst hydrogenation unstable and produces other harmful degradation products, destroying the effective components of the working fluid, and increasing the cost of anthraquinone and regenerated alumina. Therefore, in order to improve the adaptability of the catalyst under extreme working conditions, enhance the stability of production, and minimize the operating cost, a catalyst with stronger performance is urgently needed to meet market demand. Summary of the invention
[0004] Technical purpose: In order to overcome the deficiencies in the prior art, the present invention provides a method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation. The prepared palladium catalyst not only has excellent selectivity under normal operating conditions, but also produces fewer anthraquinone by-products under high-temperature conditions, greatly reducing the effects of problems such as over-hydrogenation and large temperature deviation caused by short-term deviation of the working fluid in the fixed-bed process on systems such as the palladium catalyst and the working fluid. The method has low cost and can be produced on a large scale in an industrial manner.
[0005] Technical solution: To achieve the above purpose, the present invention discloses a method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation, comprising the following steps:
[0006] Step S1: After the aluminum raw material and deionized water are mixed evenly in proportion, a fixed proportion of acid solution is added dropwise, and the reaction temperature and speed are controlled at the same time. After a certain reaction time, a colloid is obtained, and the colloid is acidic. A curing agent is added to the colloid, and after stirring evenly, it is formed in an oil column. Finally, after aging, washing, drying, and roasting processes, an alumina ball carrier is obtained;
[0007] Step S2: ultrasonically treating the prepared alumina ball carrier in deionized water, and removing water by suction filtration until there is no obvious water stain, to obtain a wet carrier;
[0008] Step S3: transferring the wet carrier obtained in step S2 to a palladium-carrying device, setting the rotation speed, spraying the palladium liquid on the carrier at a certain temperature and negative pressure, maintaining the temperature and pressure for 2 hours, and then washing with hot water until the chloride ion content is qualified, thereby obtaining a primary state of the palladium catalyst;
[0009] Step S4: drying and calcining the palladium catalyst obtained in step S3 to finally obtain the desired palladium catalyst.
[0010] Furthermore, in step S1, the mass ratio of the aluminum raw material, deionized water, acid solution and curing agent is 1:2-20:1-7:0.2-5, and is optimized to be 1:3-10:1.5-4:0.3-2.5.
[0011] Furthermore, in step S1, the reaction temperature of the material is 10-100°C, optimized to 25-95°C; the stirring rate is 50-400rad / min, optimized to 100-180rad / min; the stirring time is 0.1-12h, optimized to 0.5-8h; the oil column temperature is 60-110°C, optimized to 85-99°C; the aging temperature is 80-150°C, optimized to 85-140°C; the aging time is 1-30h, optimized to 2-24h; the washing temperature is 10-100°C, preferably 10-70°C; the drying temperature is 70-120°C, optimized to 95-115°C; the drying time is 8-24h, optimized to 14-18h; the calcination temperature is 400-1100°C, optimized to 500-1000°C; the calcination time is 1-8h, optimized to 2-6h.
[0012] Furthermore, in step S1, the aluminum raw material includes one or more of aluminum powder, pseudo-boehmite and aluminum nitrate; the acid solution includes one or more of hydrochloric acid, nitric acid, formic acid and acetic acid; the curing agent includes one or more of hexamethylenetetramine, ammonia water and urea; the oil in the oil column includes one or more of mechanical oil, hydraulic oil, gear oil and white oil.
[0013] Furthermore, in step S2, the selected specific surface area of the alumina ball carrier is 70 to 150 m 2 / g, preferably 80 to 120 m 2 / g; pore volume is 0.65-1.5cc / g, preferably 0.7-0.9cc / g; average pore diameter is 15-30nm, preferably 18-25nm; bulk density is 0.4-0.8g / cm 3 , preferably 0.45 to 0.6 g / cm 3 ; The diameter of the alumina ball carrier is 1.8 to 2.5 mm, preferably 2.2 to 2.4 mm.
[0014] Furthermore, in step S2, the volume of deionized water is 1.2 to 2 times, preferably 1.5 to 1.8 times, of the volume of the alumina ball carrier; the soaking time is 0.5 to 3 hours, preferably 1 to 2 hours; and the ultrasonic frequency is 20 to 50 khz, preferably 30 to 40 khz.
[0015] Furthermore, in step S3, the rotation speed of the palladium-carrying equipment is 2 to 10 rad / min, preferably 3 to 5 rad / min; the temperature is 70 to 99°C, preferably 80 to 90°C; the vacuum degree is 0 to -1 bar, preferably -0.1 to -0.4 bar; the palladium liquid content is 0.2wt% to 0.8wt%, preferably 0.3wt% to 0.7wt%; the ratio of the volume of the palladium liquid to the volume of the carrier is 1:2 to 4, preferably 1:2.5 to 3.5; the hot water washing temperature is 30 to 80°C, preferably 40 to 60°C.
[0016] Furthermore, in step S3, the palladium solution includes one or more of palladium chloride solution, palladium nitrate solution, and palladium acetate solution.
[0017] Furthermore, in step S4, the drying condition is drying under negative pressure, the vacuum degree is 0 to -1 bar, preferably -0.4 to -0.6 bar; the drying temperature is 90 to 140°C, optimized to 100 to 110°C; the drying time is 0.5 to 24h, optimized to 8 to 15h; the roasting temperature is 450 to 550°C, optimized to 480 to 520°C; the roasting time is 1 to 6h, optimized to 2.5 to 4h.
[0018] Furthermore, the average pore size of the palladium catalyst is 19-23 nm, and the diameter is 2.21-2.38 mm.
[0019] The present invention has the following beneficial effects:
[0020] (1) The average pore size of the palladium catalyst prepared by the present invention is 19-23 nm, and it has a large-pore mesoporous structure, and the palladium is distributed on the surface. Anthraquinone can quickly detach from the palladium catalyst after hydrogenation is completed, avoiding excessive hydrogenation, and effectively alleviating the problem of palladium catalyst clogging the pores and anthraquinone degradation caused by excessive hydrogenation under special working conditions; the diameter of the palladium catalyst is 2.21-2.38 mm, which can avoid the problem of large bed resistance caused by too small particle size, and can also avoid the problem of reduced utilization rate of the palladium catalyst caused by too large particle size;
[0021] (2) The amount of palladium required for preparing the palladium catalyst of the present invention is about 50% of the amount of palladium required for preparing the traditional palladium catalyst, the cost of precious metals is significantly reduced, but the activity can reach 95% of it, and the selectivity of the palladium catalyst under high temperature conditions is increased by more than 20%, which fully meets the production needs;
[0022] (3) In the process of preparing the alumina ball carrier of the present invention, the colloid as an intermediate product can more finely control the pore structure and surface characteristics of the alumina ball carrier, and the size and shape of the colloidal particles can be controlled by adjusting the reaction conditions (such as acid amount, temperature, rotation speed, etc.), thereby accurately regulating the pore size and distribution of the final alumina product; the colloid can evenly mix the aluminum source and other components at the molecular level due to its highly dispersed characteristics, and this uniform dispersion ensures that the active centers can be evenly distributed on the surface and inside of the alumina ball carrier during the subsequent molding and calcination process; the thermal stability is improved, and in the high-temperature catalytic reaction, the alumina ball carrier with high thermal stability can maintain its structure unchanged, maintaining the catalytic activity and service life;
[0023] (4) The role of the ultrasonic treatment in the present invention is to clean the surface of the carrier and the aluminum oxide powder attached to the micropores, reduce the loss of palladium caused by the shedding of palladium-containing aluminum oxide powder during palladium adsorption, and ensure that the water in the micropores of the carrier is evenly soaked to ensure the stability of palladium adsorption of the product;
[0024] (5) The palladium catalyst prepared by the present invention controls the vaporization of water in the carrier and quickly sprays the palladium liquid on the surface of the carrier. Due to the high temperature of the carrier surface, the evaporation of water and the negative pressure, the palladium is loaded on the surface of the carrier, so the utilization rate of the active metal is high;
[0025] (6) The palladium catalyst prepared by the present invention not only has excellent selectivity under normal operating conditions, but also produces less anthraquinone by-products under high temperature conditions, which greatly reduces the impact of problems such as over-hydrogenation and large temperature deviation caused by short-term deviation of the working fluid in the fixed bed process on the palladium catalyst and working fluid system. It has low cost and can be mass-produced industrially. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a diagram showing the isothermal adsorption and desorption of the palladium catalyst prepared in Example 1 of the present invention;
[0027] Figure 2 It is a diagram showing the isothermal adsorption and desorption of the palladium catalyst of the comparative example of the present invention;
[0028] Figure 3 This is a schematic diagram of the pore radius of the palladium catalyst prepared in Example 1 of the present invention;
[0029] Figure 4 It is a schematic diagram of the pore radius of the palladium catalyst in the comparative example of the present invention;
[0030] Figure 5 The working solution was analyzed by liquid chromatography for effective anthraquinone and degradation product spectrum (I);
[0031] Figure 6 The working solution was analyzed by liquid chromatography to obtain the spectrum of effective anthraquinone and degradation products (II). DETAILED DESCRIPTION
[0032] The following is combined with Figure 1 To Attachment Figure 6 The principles and features of the present invention are described, and the examples given are only used to explain the present invention, rather than to limit the scope of the present invention.
[0033] Embodiment 1:
[0034] A method for preparing a palladium catalyst with low palladium content and high selectivity for anthraquinone hydrogenation in a fixed bed, comprising the following steps:
[0035] Step S1: 100g of aluminum powder is added to 500g of deionized water, and 250g of 30% nitric acid is added dropwise at a rate of 20ml / min, and mixed and stirred at a stirring rate of 80rad / min in a reflux bottle at 80°C. After stirring for 6h, the mixture is cooled to room temperature to obtain a colloid, which is acidic. 40g of ammonia water and 10g of urea are added, and mixed and stirred at a stirring rate of 150rad / min. After stirring for 0.5h, the mixture is formed in a white oil column at 90°C, reacted at 120°C for 4h, washed and degreased, dried at 110°C, and calcined at 900°C for 4h to obtain an alumina ball carrier;
[0036] Step S2: Take 100g of carrier, add 150ml of deionized water, ultrasonically treat at 40khz for 30min, and then filter until there is no obvious water to obtain a wet carrier;
[0037] Step S3: transfer the wet carrier to a palladium-carrying device and heat it to 90°C, weigh 0.234g of palladium chloride, add 20ml of water, add 0.3g of hydrochloric acid and 0.5g of sodium chloride, heat to dissolve, cool and dilute with water to 70ml to obtain palladium liquid, the rotation speed is 3rad / min, wait for the kettle to be preheated to 90°C, spray the palladium liquid onto the carrier, and after completion, control the temperature to 80°C, the vacuum degree to -0.3bar, continue to rotate for 2h, and then wash with 60°C deionized water until the chloride ion is less than 10mg / L to obtain the primary state of palladium catalyst;
[0038] Step S4: Control the rotation speed to 4 rad / min, vacuum degree to -0.8 bar, and dry at 120°C for 12 h. The calcination atmosphere is air. The temperature is raised to 450°C at 5°C / min. The calcination time is 3 h to obtain a Pd / Al2O3 catalyst. The palladium content in the Pd / Al2O3 catalyst is 1.4 wt‰.
[0039] Embodiment 2:
[0040] A method for preparing a palladium catalyst with low palladium content and high selectivity for anthraquinone hydrogenation in a fixed bed, comprising the following steps:
[0041] Step S1: 100g of aluminum powder is added to 400g of water, and 340g of 30% hydrochloric acid is added dropwise at a rate of 3ml / min, and mixed and stirred at a stirring rate of 100rad / min in a reflux bottle at 80°C. After stirring for 6h, the mixture is cooled to room temperature to obtain a colloid, which is acidic. 30g of hexamethylenetetramine and 10g of urea are added, and mixed and stirred at a stirring rate of 150rad / min. After stirring for 0.5h, the mixture is formed in a white oil column at 92°C, reacted at 140°C for 10h, washed and degreased, dried at 110°C, and calcined at 900°C for 4h to obtain an alumina ball carrier;
[0042] Step S2: Take 100g of carrier, add 150ml of deionized water, ultrasonically treat at 40khz for 30min, and then filter until there is no obvious water to obtain a wet carrier;
[0043] Step S3: transfer the wet carrier to a palladium-carrying device and heat it to 90°C, weigh 0.268g of palladium chloride, add 20ml of water, add 0.34g of hydrochloric acid and 0.57g of sodium chloride, heat to dissolve, cool and dilute with water to 75ml to obtain palladium liquid, the rotation speed is 3rad / min, wait for the kettle to be preheated to 90°C, spray the palladium liquid onto the carrier, and after completion, control the temperature to 80°C, the vacuum degree to -0.3bar, continue to rotate for 2h, and then wash with 60°C deionized water until the chloride ion is less than 10mg / L to obtain the primary state of palladium catalyst;
[0044] Step S4: Control the rotation speed to 4 rad / min, vacuum degree to -0.8 bar, and dry at 120°C for 12 hours. The calcination atmosphere is air, and the temperature is increased to 450°C at 5°C / min. The calcination time is 3 hours to obtain a Pd / Al2O3 catalyst, wherein the palladium content in the Pd / Al2O3 catalyst is 1.6wt‰.
[0045] Embodiment 3:
[0046] A method for preparing a palladium catalyst with low palladium content and high selectivity for anthraquinone hydrogenation in a fixed bed, comprising the following steps:
[0047] Step S1: 300 g of pseudo-boehmite is added to 500 g of deionized water, and 400 g of 10% nitric acid is added. After mixing evenly, the mixture is stirred at 50° C. at a stirring rate of 150 rad / min. After stirring for 0.5 h, a colloid is obtained. The colloid is acidic. 28 g of urea and 80 g of hexamethylenetetramine are added, and the mixture is stirred evenly for 30 min. The mixture is formed in a white oil column at 88° C., reacted at 110° C. for 2 h, washed and degreased, dried at 110° C., and calcined at 900° C. for 4 h to obtain an alumina ball carrier.
[0048] Step S2: Take 100g of carrier, add 150ml of deionized water, ultrasonically treat at 40khz for 30min, and then filter until there is no obvious water to obtain a wet carrier;
[0049] Step S3: transfer the wet carrier to a palladium-carrying device and heat it to 90°C, weigh 0.44g of palladium nitrate, add 20ml of water, add 1g of nitric acid and heat to dissolve, cool and dilute with water to 65ml to obtain palladium liquid, the rotation speed is 3rad / min, wait for the kettle to be preheated to 90°C, spray the palladium liquid onto the carrier, and after completion, control the temperature to 80°C, the vacuum degree to -0.3bar, continue to rotate for 2h, and then wash with 60°C deionized water until the chloride ion is less than 10mg / L to obtain the primary state of palladium catalyst;
[0050] Step S4: drying at 120°C for 12 hours under a controlled rotation speed of 4 rad / min and a vacuum degree of -0.8 bar, with air as the calcination atmosphere, heating to 450°C at a rate of 5°C / min, and calcination time of 3 hours to obtain a Pd / Al2O3 catalyst having a palladium content of 1.8 wt‰.
[0051] Comparative Example: A commercially available palladium catalyst was used, and its palladium content was 3 wt‰.
[0052] The palladium catalysts in Examples 1-3 and Comparative Examples are now tested. The specific testing method is as follows: 20 g of palladium catalyst is loaded, 200 ml of working solution is circulated (the working solution component solvent is Ar:TOP:TBU=2:0.7:0.3, the solute is diethyl anthraquinone, and the concentration is 60 g / L), the operating temperature is 70°C, the circulation volume is 1.8 L / h, and the activity value is 5 ml of working solution is taken every 3 hours, and then the activity data is obtained by titration with potassium permanganate and the average value is taken. The selectivity evaluation is to use liquid chromatography to detect the components of the working solution after running for 24 hours, and the degradation is judged according to the anthraquinone content and impurity peaks. The specific data are shown in Table 1:
[0053] Table 1: Summary of Examples 1-3 and Comparative Examples
[0054]
[0055]
[0056] in conclusion:
[0057] (1) It can be seen from the data in Table 1 that the activity of the palladium catalysts in the three examples is more than 95% of that of the 3‰ palladium catalyst in the comparative example, the total anthraquinone content is more than 20% higher, and the anthraquinone degradation is less;
[0058] (2) Figure 1 and Figure 2 The isothermal adsorption and desorption diagrams of the palladium catalyst prepared in Example 1 and the comparative example palladium catalyst are shown in red and black, respectively. Since Examples 1-3 show the same trend, Example 1 is used for overall analysis. Figure 1 It can be seen that: Example 1 is a typical ordered mesoporous material, and the pressure at the tail end condensation section is relatively large, indicating that the palladium catalyst mesopores are evenly distributed and have a large pore size. The comparative example is also a typical ordered mesoporous material, but the pressure at the tail end condensation section is lower than that of the example, indicating that the palladium catalyst mesopores are evenly distributed, but the pore size is small;
[0059] (3) Figure 3 and Figure 4 The desorption pore area distribution diagrams of the palladium catalyst prepared in Example 1 and the palladium catalyst of the comparative example are shown respectively. Since Examples 1-3 show the same trend, Example 1 is used for overall analysis. Figure 3 It can be seen that the pore size of the palladium catalyst in Example 1 is concentrated between 18 and 22 nm, and the pore size of the palladium catalyst in the comparative example is concentrated between 7 and 9 nm;
[0060] (4) Figure 5 and Figure 6After the working solution was run for a period of time under the specified conditions in Example 1 and the comparative example, the effective anthraquinone and degradation product spectra were analyzed by liquid chromatography. Since Examples 1-3 showed the same trend, Example 1 was used for overall analysis. According to the peak shape, it can be seen that after the working solution and the palladium catalyst were run at 70° C. for 24 hours, the anthraquinone in the working solution corresponding to Example 1 was mainly diethyl anthraquinone and tetrahydrodiethyl anthraquinone, both of which were effective components, after liquid chromatography detection; while there were two obvious impurity peaks in the working solution corresponding to the comparative example. Combined with the total anthraquinone detection data, it was concluded that the comparative example had more degradation products after running at high temperature, so it can be proved that the performance of Example 1 is more stable.
[0061] The palladium catalyst prepared by the present invention not only has excellent selectivity under normal operating conditions, but also has less anthraquinone by-products under high temperature conditions, which greatly reduces the impact of problems such as over-hydrogenation and large temperature deviation caused by short-term deviation of the working fluid in the fixed bed process on the palladium catalyst and the working fluid system. The cost is low and can be mass-produced industrially.
[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a palladium catalyst with low palladium content and high selectivity for anthraquinone hydrogenation in a fixed bed, It is characterized in that The following steps are involved: Step S1: After the aluminum raw material and deionized water are mixed evenly in proportion, a fixed proportion of acid solution is added dropwise, and the reaction temperature and speed are controlled at the same time. After a certain reaction time, a colloid is obtained, and the colloid is acidic. A curing agent is added to the colloid, and after stirring evenly, it is formed in an oil column. Finally, after aging, washing, drying, and roasting processes, an alumina ball carrier is obtained; Step S2: ultrasonically treating the prepared alumina ball carrier in deionized water, and removing water by suction filtration until there is no obvious water stain, to obtain a wet carrier; Step S3: transferring the wet carrier obtained in step S2 to a palladium-carrying device, setting the rotation speed, spraying the palladium liquid on the carrier at a certain temperature and negative pressure, maintaining the temperature and pressure for 2 hours, and then washing with hot water until the chloride ion content is qualified, thereby obtaining a primary state of the palladium catalyst; Step S4: drying and calcining the palladium catalyst obtained in step S3 to finally obtain the desired palladium catalyst.
2. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation according to claim 1, Features: In step S1, the mass ratio of the aluminum raw material, deionized water, acid solution and curing agent is 1:2-20:1-7:0.2-5, and is optimized to be 1:3-10:1.5-4:0.3-2.
5.
3. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for anthraquinone hydrogenation in a fixed bed according to claim 1, Features: In step S1, the reaction temperature of the material is 10-100°C, optimized to 25-95°C; the stirring rate is 50-400rad / min, optimized to 100-180rad / min; the stirring time is 0.1-12h, optimized to 0.5-8h; the oil column temperature is 60-110°C, optimized to 85-99°C; the aging temperature is 80-150°C, optimized to 85-140°C; the aging time is 1-30h, optimized to 2-24h; the washing temperature is 10-100°C, preferably 10-70°C; the drying temperature is 70-120°C, optimized to 95-115°C; the drying time is 8-24h, optimized to 14-18h; the calcination temperature is 400-1100°C, optimized to 500-1000°C; the calcination time is 1-8h, optimized to 2-6h.
4. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation according to claim 1, Features: In step S1, the aluminum raw material includes one or more of aluminum powder, pseudo-boehmite and aluminum nitrate; the acid solution includes one or more of hydrochloric acid, nitric acid, formic acid and acetic acid; the curing agent includes one or more of hexamethylenetetramine, ammonia water and urea; the oil in the oil column includes one or more of mechanical oil, hydraulic oil, gear oil and white oil.
5. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation according to claim 1, Features: In step S2, the selected specific surface area of the alumina ball carrier is 70 to 150 m 2 / g, preferably 80 to 120 m 2 / g; pore volume is 0.65-1.5cc / g, preferably 0.7-0.9cc / g; average pore diameter is 15-30nm, preferably 18-25nm; bulk density is 0.4-0.8g / cm 3 , preferably 0.45 to 0.6 g / cm 3 ; The diameter of the alumina ball carrier is 1.8 to 2.5 mm, preferably 2.2 to 2.4 mm.
6. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation according to claim 1, Features: In step S2, the volume of deionized water is 1.2 to 2 times, preferably 1.5 to 1.8 times, the volume of the alumina ball carrier; the soaking time is 0.5 to 3 hours, preferably 1 to 2 hours; the ultrasonic frequency is 20 to 50 khz, preferably 30 to 40 khz.
7. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation according to claim 1, Features: In step S3, the rotation speed of the palladium-carrying equipment is 2 to 10 rad / min, preferably 3 to 5 rad / min; the temperature is 70 to 99°C, preferably 80 to 90°C; the vacuum degree is 0 to -1 bar, preferably -0.1 to -0.4 bar; the palladium liquid content is 0.2wt% to 0.8wt%, preferably 0.3wt% to 0.7wt%; the ratio of the palladium liquid volume to the carrier volume is 1:2 to 4, preferably 1:2.5 to 3.5; the hot water washing temperature is 30 to 80°C, preferably 40 to 60°C.
8. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation according to claim 1, Features: In step S3, the palladium solution includes one or more of palladium chloride solution, palladium nitrate solution, and palladium acetate solution.
9. The method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation according to claim 1, Features: In step S4, the drying condition is drying under negative pressure, the vacuum degree is 0 to -1 bar, preferably -0.4 to -0.6 bar; the drying temperature is 90 to 140°C, optimized to 100 to 110°C; the drying time is 0.5 to 24h, optimized to 8 to 15h; the roasting temperature is 450 to 550°C, optimized to 480 to 520°C; the roasting time is 1 to 6h, optimized to 2.5 to 4h.
10. The method for preparing a palladium catalyst with low palladium content and high selectivity for anthraquinone hydrogenation in a fixed bed according to claim 1, Features: The average pore size of the palladium catalyst is 19-23 nm, and the diameter thereof is 2.21-2.38 mm.
Citation Information
Patent Citations
Method for preparing hydrogen peroxide by adding hydrogen in anthraquinone
CN102219189A
Supported catalyst and preparation method thereof
CN104001557A
Preparation method of loaded type palladium-alumina catalyst
CN106902815A
Palladium catalyst for producing hydrogen peroxide by anthraquinone process and preparation method of palladium catalyst
CN110639512A
Rare-earth-doped spherical alumina Pd-based catalyst as well as preparation method and application thereof
CN113600157A