Catalyst forming body as well as preparation method and application thereof
By molding the catalyst powder with a filler and a neutral silica sol solution, a catalyst molded body with high mechanical strength and catalytic stability was prepared, and the problem of insufficient stability and reactivity of the catalyst molded body in the prior art was solved. The industrial application prospects of ethanol-catalyzed dehydrogenation to produce acetaldehyde have been realized.
Patent Information
- Application Number
- CN202411054076.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art lacks catalyst molded bodies with good mechanical strength, high reactivity and good stability, which limits the industrial application of ethanol catalytic dehydrogenation to produce acetaldehyde.
By mixing the catalyst powder with a filler and molding and heat treatment with a neutral silicon sol solution, a catalyst molded body with excellent mechanical strength and high catalytic stability is prepared, and a combination of copper oxide and other metal oxides is used to combine the adhesive. Neutral silica sol maintains high activity of Cu and improves overall stability.
The prepared catalyst molded body exhibits high conversion and selectivity in the acetaldehyde reaction of ethanol without oxygen catalytic dehydrogenation, and can operate continuously and stably for at least 300 hours in a fixed bed reactor, with excellent mechanical strength and resistance. Abrasive.
Smart Images

Figure CN118976492A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a catalyst forming body and a preparation method and application thereof. Background Art
[0002] Solid catalyst moldings are used in most industrial catalytic processes. In the production of solid catalyst moldings, catalyst molding technology plays a core role. Common molding technologies include compression molding, extrusion molding, rotational molding, pressure molding, spherical molding and spray molding. The structure and parameters of the catalyst molding have an important influence on the catalytic reaction: (1) Different catalyst moldings, especially the shape of the moldings, have an important influence on the heat distribution and stable operation of industrial equipment; (2) For fixed bed reactors, the molding parameters of the catalyst molding have a significant impact on the catalyst activity selectivity and the fixed bed pressure drop; (3) For reaction processes with long reaction cycles and high reaction space velocities, higher requirements are placed on the strength and wear resistance of the catalyst molding.
[0003] The preparation of acetaldehyde by catalytic dehydrogenation of ethanol without oxygen is an ideal process route. This process is an atom-economic reaction. It produces acetaldehyde and produces high-purity hydrogen as a by-product. At the same time, this process can be realized by a fixed bed reactor, which has the obvious advantages of small equipment investment and simple operation process. Existing literature and technology on the catalytic dehydrogenation process of ethanol mainly focus on the study of catalytic mechanism and reaction activity. At present, there is no report on industrial process. This is mainly because there is a lack of catalyst moldings with good mechanical strength, high reaction activity and good stability, which limits its industrial application. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a catalyst molding and its preparation method and application. The catalyst molding prepared by the present invention has excellent mechanical strength, good catalytic stability and high reaction activity, which is conducive to promoting the industrialization process of ethanol catalytic dehydrogenation to acetaldehyde.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a catalyst molded body, comprising the following steps:
[0007] Mixing catalyst powder and filler to obtain mixed powder; the catalyst powder is a first metal oxide or a mixture of a first metal oxide and a second metal oxide, the first metal oxide is copper oxide, and the second metal oxide is one or more of magnesium oxide, chromium oxide, iron oxide, cobalt oxide and nickel oxide;
[0008] The mixed powder is mixed with a neutral silica sol solution, and molded and heat-treated in sequence to obtain the catalyst molded body.
[0009] Preferably, when the catalyst powder is a mixture of a first metal oxide and a second metal oxide, the mass ratio of the second metal oxide to the first metal oxide is (0.05-0.5):1.
[0010] Preferably, the filler is one or more of silicon oxide, aluminum oxide and diatomaceous earth.
[0011] Preferably, the mass content of the catalyst powder in the mixed powder is 2-15%; and the particle size of the mixed powder is 100-500 meshes.
[0012] Preferably, the mass content of SiO2 in the neutral silica sol solution is 1-10%; the mass of SiO2 in the neutral silica sol solution accounts for 2-15% of the sum of the mass of SiO2 in the mixed powder and the neutral silica sol solution.
[0013] Preferably, the forming comprises ball forming.
[0014] Preferably, the heat treatment comprises drying and calcining in sequence; the drying temperature is 90-120° C. and the time is 1-24 hours, and the calcining temperature is 200-700° C. and the time is 5-24 hours.
[0015] Preferably, the catalyst molded body has a diameter of 2 to 6 mm and a compressive strength of 20 N or more.
[0016] The present invention provides a catalyst molded body prepared by the preparation method described in the above technical solution.
[0017] The present invention provides the use of the catalyst molded body described in the above technical solution in the reaction of ethanol oxygen-free catalytic dehydrogenation to produce acetaldehyde.
[0018] The present invention provides a method for preparing a catalyst molded body, comprising the following steps: mixing catalyst powder and a filler to obtain a mixed powder; the catalyst powder is a first metal oxide or a mixture of a first metal oxide and a second metal oxide, the first metal oxide is copper oxide, and the second metal oxide is one or more of magnesium oxide, chromium oxide, iron oxide, cobalt oxide and nickel oxide; mixing the mixed powder with a neutral silica sol solution, and sequentially performing molding and heat treatment to obtain the catalyst molded body. The present invention uses copper oxide as a necessary component of the catalyst. The Cu element has good catalytic activity for ethanol dehydrogenation to acetaldehyde (copper oxide will be in situ reduced to generate nano Cu metal in the hot atmosphere of alcohol), but the Tamman temperature of Cu is low, and thermal aggregation will occur during the reaction, so that the Cu particles continue to grow and eventually lead to the deactivation of the catalyst. The present invention disperses the active component Cu element by adding a filler, especially adding other metal oxides (magnesium oxide, chromium oxide, iron oxide, cobalt oxide, nickel oxide), which can further play a role in dispersing Cu; these matching components are molded by an adhesive neutral silica sol solution, which can better maintain the high activity of Cu and the overall stability of the catalyst, and the active sites of the catalyst will not be destroyed during the molding process, which can avoid the catalytic activity of the catalyst after molding. Reduced, while making the catalyst after molding have high strength. The catalyst molded body prepared by the present invention has good catalytic stability and high reaction activity, and has excellent mechanical strength, high compressive strength, and good wear resistance, so that it has good industrial application prospects in fixed bed continuous reactors.
[0019] The present invention provides the use of the catalyst molded body described in the above technical solution in the reaction of ethanol oxygen-free catalytic dehydrogenation to acetaldehyde. The catalyst molded body described in the present invention can realize the continuous catalytic dehydrogenation of ethanol to acetaldehyde in a fixed bed reactor, and has excellent stability and catalytic performance. The results of the embodiment show that when the catalyst molded body described in the present invention is used for ethanol oxygen-free catalytic dehydrogenation to acetaldehyde, the conversion rate of ethanol is 18.2-32.6%, the acetaldehyde selectivity is 91.1-96.7%, and the reaction temperature is 220°C and the ethanol mass space velocity is 2.0h -1 Under the conditions, the catalyst molded body can continue to operate stably for not less than 300 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a photograph of the catalyst shaped body prepared in Example 1;
[0021] Figure 2 The catalyst stability test results in the examples are shown in FIG. DETAILED DESCRIPTION
[0022] The present invention provides a method for preparing a catalyst molded body, comprising the following steps:
[0023] Mixing catalyst powder and filler to obtain mixed powder; the catalyst powder is a first metal oxide or a mixture of a first metal oxide and a second metal oxide, the first metal oxide is copper oxide, and the second metal oxide is one or more of magnesium oxide, chromium oxide, iron oxide, cobalt oxide and nickel oxide;
[0024] The mixed powder is mixed with a neutral silica sol solution, and molded and heat-treated in sequence to obtain the catalyst molded body.
[0025] In the present invention, unless otherwise specified, the raw materials involved are commercially available products well known in the art.
[0026] The present invention mixes catalyst powder and filler to obtain mixed powder.
[0027] In the present invention, the catalyst powder is a first metal oxide or a mixture of a first metal oxide and a second metal oxide, the first metal oxide is copper oxide, and the second metal oxide is one or more of magnesium oxide, chromium oxide, iron oxide, cobalt oxide and nickel oxide. In the present invention, when the catalyst powder is a mixture of a first metal oxide and a second metal oxide, the mass ratio of the second metal oxide to the first metal oxide is preferably (0.05-0.5):1, specifically 0.05:1, 0.07:1, 0.08:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1. In the present invention, the filler is preferably one or more of silicon oxide, aluminum oxide and diatomaceous earth.
[0028] In the present invention, the mass content of the catalyst powder in the mixed powder is preferably 2-15%, more preferably 4-10%, and further preferably 5-10%. In the present invention, the particle size of the mixed powder is preferably 100-500 mesh, more preferably 200-400 mesh, and further preferably 300 mesh. In the present invention, the catalyst powder and the filler are preferably mixed uniformly and then crushed to obtain the mixed powder of the particle size.
[0029] The present invention uses copper oxide as an essential component of the catalyst. The Cu element has good catalytic activity for ethanol dehydrogenation to acetaldehyde (copper oxide will be in-situ reduced to generate nano Cu metal in the hot atmosphere of alcohol). However, the Tamman temperature of Cu is relatively low, and thermal aggregation will occur during the reaction process, so that Cu particles continue to grow and eventually lead to catalyst deactivation. The present invention disperses the active component Cu element by adding a filler, especially by adding other metal oxides (magnesium oxide, chromium oxide, iron oxide, cobalt oxide, nickel oxide), which can further disperse Cu and ensure the high activity of the catalyst.
[0030] After obtaining the mixed powder, the present invention mixes the mixed powder with a neutral silica sol solution, and sequentially performs molding and heat treatment to obtain the catalyst molded body.
[0031] In the present invention, the mass content of the neutral silica sol solution is preferably 1-10%, more preferably 6-8%, and further preferably 3-5%; in an embodiment of the present invention, the neutral silica sol solution is preferably prepared by adding water to a commercially available neutral silica sol (i.e., an aqueous dispersion of nano-silicon dioxide, pH=6-8). In the present invention, the mass of SiO2 in the neutral silica sol solution accounts for 2-15%, preferably 10-14%, of the sum of the mass of SiO2 in the mixed powder and the neutral silica sol solution. In the present invention, the neutral silica sol solution is used as an adhesive, and the main component of the neutral silica sol solution is SiO2, and no other components are additionally introduced, so there is no negative impact on the reaction performance of the catalyst molding.
[0032] In the present invention, the molding preferably includes ball forming, and the ball forming is preferably performed using a disc ball machine or a coating machine. The present invention has no special requirements for the disc ball machine or the coating machine, and the corresponding mechanical equipment familiar to those skilled in the art can be used. In the present invention, the size and compressive strength of the molded body can be regulated by controlling the amount of feed, the ball time, the angle of the ball equipment, and the concentration and addition amount of the neutral silica sol solution during the ball forming process. In the present invention, it is preferred that small spheres with a diameter of 2 to 6 mm (preferably 3 to 5 mm) are obtained by the ball forming, and the compressive strength of each small sphere is preferably above 20N, more preferably 50 to 70N, that is, the parameter setting of the ball forming is guaranteed to obtain a molded body of the size and compressive strength.
[0033] In the present invention, the heat treatment preferably includes drying and calcining in sequence. In the present invention, the drying temperature is preferably 90-120°C, more preferably 100-120°C, the time is preferably 1-24h, more preferably 3-8h; the function of the drying is to remove the main moisture in the material after molding. In the present invention, the calcining temperature is preferably 200-700°C, more preferably 400-500°C, the time is preferably 5-24h, more preferably 5-8h; the calcining process is mainly the bonding of the adhesive silicon oxide and the carrier (i.e., filler), which plays a role in molding aging and makes the catalyst thermally more stable. The present invention performs drying and calcining of the molded body in stages under different temperature conditions, and the mechanical strength of the catalyst molded body can be improved by adjusting the removal rate of moisture and the like.
[0034] The catalyst powder of the present invention has high activity for catalytic dehydrogenation of ethanol, and the introduction of neutral silica sol as an adhesive does not change the acidity and alkalinity of the original catalyst, thereby ensuring the activity of the catalyst after molding and avoiding reduction in the catalytic activity of the catalyst after molding.
[0035] The present invention provides a catalyst molded body prepared by the preparation method described in the above technical solution. In the present invention, the catalyst molded body is preferably spherical, the diameter of a single sphere is preferably 2 to 6 mm, and the compressive strength is preferably above 20 N. The catalyst molded body provided by the present invention has excellent mechanical strength, good catalytic stability and high reaction activity.
[0036] The present invention provides the use of the catalyst molded body described in the above technical solution in the reaction of ethanol oxygen-free catalytic dehydrogenation to acetaldehyde. In the present invention, the reaction temperature is preferably 220-280°C, more preferably 220-240°C, and the mass space velocity of ethanol is preferably 1.0-3.0h -1 , more preferably 2.0h -1 . During the reaction, ethanol undergoes a dehydrogenation reaction under the catalytic action of the catalyst molded body to produce acetaldehyde and hydrogen as a by-product. In the present invention, the reaction is preferably carried out in a fixed bed reactor, specifically, the catalyst molded body is loaded into a fixed bed reactor, ethanol vapor is introduced, and the reaction is continuously carried out at 220 to 280° C. to obtain a reaction liquid containing an acetaldehyde product. The present invention applies the catalyst molded body to the catalytic dehydrogenation of ethanol to produce acetaldehyde, has excellent stability and catalytic performance, and is conducive to promoting the industrialization of the catalytic dehydrogenation of ethanol to produce acetaldehyde.
[0037] In order to further illustrate the present invention, the catalyst molded body provided by the present invention and its preparation method and application are described in detail below in conjunction with examples, but they should not be construed as limiting the scope of protection of the present invention.
[0038] Example 1
[0039] The preparation steps of the catalyst molding are as follows:
[0040] 10 g of copper oxide catalyst powder and 90 g of diatomaceous earth powder were fully mixed and crushed into 300 mesh size to obtain a mixed powder;
[0041] Prepare 120 g of a neutral silica sol solution with a concentration of 10 wt % (i.e., SiO2 mass content) as an adhesive;
[0042] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 5 hours to form small balls of about 3 mm in size;
[0043] The formed pellets were dried at 100°C for 5 hours and then calcined at 500°C for 5 hours to obtain a catalyst formed body.
[0044] Figure 1 This is a photograph of the catalyst shaped body prepared in Example 1.
[0045] Example 2
[0046] The preparation steps of the catalyst molding are as follows:
[0047] 14 g of copper oxide, 1 g of magnesium oxide catalyst powder and 85 g of aluminum oxide powder were fully mixed and crushed into a 300 mesh size to obtain a mixed powder;
[0048] Prepare 300 g of a neutral silica sol solution with a concentration of 5 wt% (i.e., SiO2 mass content) as an adhesive;
[0049] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 12 hours to form small balls of about 5 mm in size;
[0050] The formed pellets were dried at 100°C for 8 hours and then calcined at 400°C for 8 hours to obtain a catalyst formed body.
[0051] Example 3
[0052] The preparation steps of the catalyst molding are as follows:
[0053] 4.5 g of copper oxide, 0.5 g of chromium oxide catalyst powder and 95 g of silicon oxide powder were fully mixed and crushed into a size of 300 mesh to obtain a mixed powder;
[0054] Prepare 200 g of a neutral silica sol solution with a concentration of 6 wt % (i.e., SiO2 mass content) as an adhesive;
[0055] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 8 hours to form small balls of about 4 mm in size;
[0056] The formed pellets were dried at 120°C for 3 hours and then calcined at 700°C for 5 hours to obtain a catalyst formed body.
[0057] Example 4
[0058] The preparation steps of the catalyst molding are as follows:
[0059] 4 g of copper oxide catalyst powder and 96 g of silicon oxide powder were fully mixed and crushed into 300 mesh size to obtain a mixed powder;
[0060] Prepare 200 g of a neutral silica sol solution with a concentration of 8 wt % (i.e., SiO2 mass content) as an adhesive;
[0061] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 8 hours to form small balls of about 5 mm in size;
[0062] The formed pellets were dried at 100°C for 5 hours and then calcined at 500°C for 5 hours to obtain a catalyst formed body.
[0063] Example 5
[0064] The preparation steps of the catalyst molding are as follows:
[0065] 9 g of copper oxide, 1 g of nickel oxide catalyst powder and 90 g of aluminum oxide powder were fully mixed and crushed into a 300 mesh size to obtain a mixed powder;
[0066] Prepare 300 g of a neutral silica sol solution with a concentration of 5 wt% (i.e., SiO2 mass content) as an adhesive;
[0067] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 12 hours to form small balls of about 6 mm in size;
[0068] The formed pellets were dried at 100°C for 5 hours and then calcined at 500°C for 5 hours to obtain a catalyst formed body.
[0069] Example 6
[0070] The preparation steps of the catalyst molding are as follows:
[0071] 9 g of copper oxide, 1 g of iron oxide catalyst powder and 90 g of silicon oxide powder were fully mixed and crushed into a size of 300 mesh to obtain a mixed powder;
[0072] Prepare 300 g of a neutral silica sol solution with a concentration of 5 wt% (i.e., SiO2 mass content) as an adhesive;
[0073] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 12 hours to form small balls of about 5 mm in size;
[0074] The formed pellets were dried at 100°C for 5 hours and then calcined at 500°C for 5 hours to obtain a catalyst formed body.
[0075] Example 7
[0076] The preparation steps of the catalyst molding are as follows:
[0077] 9 g of copper oxide, 1 g of cobalt oxide catalyst powder and 90 g of silicon oxide powder were fully mixed and crushed into a size of 300 mesh to obtain a mixed powder;
[0078] Prepare 300 g of a neutral silica sol solution with a concentration of 5 wt% (i.e., SiO2 mass content) as an adhesive;
[0079] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 12 hours to form small balls of about 5 mm in size;
[0080] The formed pellets were dried at 100°C for 5 hours and then calcined at 500°C for 5 hours to obtain a catalyst formed body.
[0081] Comparative Example 1
[0082] The preparation steps of the catalyst molding are as follows:
[0083] 10 g of copper oxide catalyst powder and 90 g of diatomaceous earth powder were fully mixed and crushed into 300 mesh size to obtain a mixed powder;
[0084] Prepare 120 g of alkaline silica sol solution with a concentration of 10 wt % (i.e., SiO2 mass content) as an adhesive;
[0085] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 5 hours to form small balls of about 3 mm in size;
[0086] The formed pellets were dried at 100°C for 5 hours and then calcined at 500°C for 5 hours to obtain a catalyst formed body.
[0087] Comparative Example 2
[0088] The preparation steps of the catalyst molding are as follows:
[0089] 10 g of copper oxide catalyst powder and 90 g of silicon oxide powder were fully mixed and crushed into 300 mesh size to obtain a mixed powder;
[0090] Prepare 100 g of 0.2 wt% dilute nitric acid solution as an adhesive;
[0091] The mixed powder and adhesive are mixed and molded using a disc ball rolling machine, the disc ball rolling machine has an inclination angle of 45° and a rotation speed of 18 r / min, and the material is continuously rolled for 5 hours to form small balls of about 3 mm in size;
[0092] The formed pellets were dried at 100°C for 5 hours and then calcined at 500°C for 5 hours to obtain a catalyst formed body.
[0093] Performance Testing
[0094] 100 g of each catalyst molded body of the above examples were taken and loaded into a reactor. After the temperature was raised to a reaction temperature of 240° C., ethanol liquid was introduced at a flow rate of 5 mL / min. After preheating and gasification, a dehydrogenation reaction was carried out through the catalyst bed. The reaction effect was tested for 24 hours. The test results are shown in Table 1.
[0095] Table 1 Catalytic performance test results of the catalyst molded bodies of the embodiments and comparative examples
[0096]
[0097]
[0098] The stability test of the catalyst molded body of Example 3 was carried out on a fixed bed. The reaction temperature of the ethanol catalytic dehydrogenation reaction was 220° C. and the ethanol mass space velocity was 2.0 h -1 It was found that the catalyst molded body could operate stably for at least 300 hours, the average conversion rate of ethanol was 25.8%, the average selectivity of acetaldehyde was 94.8%, and other by-products included ether, ethyl acetate, butyraldehyde and n-butanol, such as Figure 2 As shown ( Figure 2 Con represents conversion rate, Sel represents selectivity, and since the selectivity of ether is very low, its corresponding curve is close to the X-axis).
[0099] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a catalyst molded body, characterized in that: The following steps are involved: Mixing catalyst powder and filler to obtain mixed powder; the catalyst powder is a first metal oxide or a mixture of a first metal oxide and a second metal oxide, the first metal oxide is copper oxide, and the second metal oxide is one or more of magnesium oxide, chromium oxide, iron oxide, cobalt oxide and nickel oxide; The mixed powder is mixed with a neutral silica sol solution, and molded and heat-treated in sequence to obtain the catalyst molded body.
2. The preparation method according to claim 1, characterized in that: When the catalyst powder is a mixture of a first metal oxide and a second metal oxide, the mass ratio of the second metal oxide to the first metal oxide is (0.05-0.5):
1.
3. The preparation method according to claim 1, characterized in that: The filler is one or more of silicon oxide, aluminum oxide and diatomaceous earth.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The mass content of the catalyst powder in the mixed powder is 2-15%; the particle size of the mixed powder is 100-500 meshes.
5. The preparation method according to claim 1, characterized in that: The mass content of SiO2 in the neutral silica sol solution is 1-10%; the mass of SiO2 in the neutral silica sol solution accounts for 2-15% of the sum of the mass of SiO2 in the mixed powder and the neutral silica sol solution.
6. The preparation method according to claim 1, characterized in that: The forming includes ball rolling forming.
7. The preparation method according to claim 1 or 6, characterized in that: The heat treatment includes drying and calcining in sequence; the drying temperature is 90-120° C. and the time is 1-24 hours; the calcining temperature is 200-700° C. and the time is 5-24 hours.
8. The preparation method according to claim 7, characterized in that: The catalyst molded body has a diameter of 2 to 6 mm and a compressive strength of more than 20 N.
9. A catalyst molded body obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the catalyst molded body according to claim 9 in the reaction of producing acetaldehyde by catalytic dehydrogenation of ethanol without oxygen.
Citation Information
Patent Citations
Extruded molding method for silica-supported copper oxide catalyst
CN109092308A
Copper-based catalyst for the conversion of ethanol to acetaldehyde by dehydrogenation and preparing method of the same
KR1020120073998A
Cited By
A method for molding calcium fluoride, a calcium fluoride molded body
CN120662256B