Beneficiation reagent for nickel flotation of ferronickel ore and preparation method of beneficiation reagent
By using ore dressing agents composed of 1,5-pentadithiol, 4-diethylaminebenzaldehyde and other minerals in the nickel-cobalt ore flotation process, the adsorption performance of nickel is improved and the nickel concentrate grade in the prior art is solved The problems of low and low recovery rates have achieved efficient nickel recycling and optimized utilization of resources.
Patent Information
- Application Number
- CN202411046089.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing nickel-cobalt ore flotation process, collectors are difficult to meet the design requirements, resulting in low nickel concentrate grade and low concentrate recovery rate, resulting in waste of mineral resources.
The ore dressing agent consisting of 1,5-pentadithiol, 4-diethylaminebenzaldehyde, activator (ammonium metatungstate), 2,7-octadienol, etc., is adopted to pass specific preparation and treatment steps Form a mixture of oily liquid and aqueous solution to improve the chemical adsorption and physical adsorption properties of nickel.
It achieves the effect of high selection efficiency and high yield of nickel metals, and is suitable for the application of nickel flotation of nickel cobalt ore, and simplifies the preparation process of ore dressing agents and reduces the dosage of agents.
Smart Images

Figure BDA0004973524250000061 
Figure BDA0004973524250000062 
Figure BDA0004973524250000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flotation reagents, and in particular discloses a flotation reagent for nickel in nickel-iron ore and a preparation method thereof. Background Art
[0002] my country's nickel raw materials mainly exist in nickel sulfide deposits, copper-nickel deposits, nickel-cobalt ore, magnesium silicate nickel ore, laterite ore, etc. Flotation is one of the methods for beneficiating nickel-cobalt ores. Sometimes, in order to improve the quality of nickel concentrate and remove impurities, the nickel concentrate needs to be subjected to chemical beneficiation treatment before flotation.
[0003] In the current nickel-cobalt ore flotation process, the dominant collectors are xanthates, sulfur-nitrogen, phosphates, xanthate esters, black esters and other flotation agents. However, in actual mineral processing, the results of using these agents often cannot meet the design requirements. The nickel concentrate product contains excessive impurities, the nickel concentrate grade is low, and the concentrate recovery rate is low, resulting in a waste of mineral resources. Summary of the invention
[0004] The invention provides a ore dressing agent for flotation of nickel from nickel-iron ore with high separation efficiency and high yield and a preparation method thereof.
[0005] To achieve the above purpose, the present invention discloses a ore dressing agent for flotation of nickel from nickel-iron ore, which is characterized in that it is made of the following raw materials in parts by weight: 5-12 parts of 1,5-pentanedithiol, 15-25 parts of sodium carbonate, 20-30 parts of sodium acetate, 20-25 parts of sodium pyrophosphate, 12-20 parts of 2,2-dihydroxymethylbutyric acid, 3-5 parts of quicklime, 40-60 parts of 4-diethylaminobenzaldehyde, 4-5 parts of activator, and 20-40 parts of 2,7-octadienol.
[0006] In the technical solution of a ore dressing agent for flotation of nickel from nickel iron ore of the present invention, the further preferred technical solution features are:
[0007] 1. Made from the following raw materials in parts by weight: 5 parts of 1,5-pentanedithiol, 15 parts of sodium carbonate, 20 parts of sodium acetate, 20 parts of sodium pyrophosphate, 12 parts of 2,2-dihydroxymethylbutyric acid, 3 parts of quicklime, 40 parts of 4-diethylaminobenzaldehyde, 4 parts of activator, and 20 parts of 2,7-octadienol;
[0008] 2. Made from the following raw materials in parts by weight: 12 parts of 1,5-pentanedithiol, 25 parts of sodium carbonate, 30 parts of sodium acetate, 25 parts of sodium pyrophosphate, 20 parts of 2,2-dihydroxymethylbutyric acid, 5 parts of quicklime, 60 parts of 4-diethylaminobenzaldehyde, 5 parts of activator, and 40 parts of 2,7-octadienol;
[0009] 3. Made from the following raw materials in parts by weight: 9 parts of 1,5-pentanedithiol, 20 parts of sodium carbonate, 25 parts of sodium acetate, 23 parts of sodium pyrophosphate, 16 parts of 2,2-dihydroxymethylbutyric acid, 4 parts of quicklime, 50 parts of 4-diethylaminobenzaldehyde, 4.5 parts of activator, and 30 parts of 2,7-octadienol;
[0010] 4. The activator is 4-terpene alcohol;
[0011] 5. The 1,5-pentanedithiol is prepared by the following method: Mix the following raw materials in parts by weight, 1 part of 3-hexyne, 1 part of hydrobromic acid and 2 parts of sodium hydrosulfide, and heat to 400°C;
[0012] The method for preparing a nickel ore dressing agent for flotation of nickel iron ore of the present invention comprises the following steps:
[0013] ⑴Weigh the raw materials by weight;
[0014] ⑵ Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare an oily solution A with a volume percentage of 30% to 65%;
[0015] ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir and react for 30-40 minutes to obtain solution B;
[0016] (4) Add 4-diethylaminobenzaldehyde, an activator, 2,7-octadienol and sodium acetate to solution B, stir the reaction at a temperature of 35°C to 65°C for 30 to 60 minutes, and then filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 30% to 70%, and the weight percentage of the aqueous solution is 30% to 70%;
[0017] ⑸Evaporate the filtrate to a specific gravity of 2.64-4.37 g / cm 3 After that, cool to 5-30°C and filter the coolant for 45-100 minutes to obtain the product.
[0018] In the technical solution of the method for preparing a nickel-iron ore flotation nickel dressing agent of the present invention, the further preferred technical solution features are:
[0019] 1. In step (3), the reaction was stirred for 35 min at a stirring speed of 105 rpm;
[0020] 2. In step (4), the temperature is 50°C, the stirring reaction time is 45 min, and the stirring rate is 80 rpm;
[0021] 3. In step (5), the cooling method adopts gradient cooling, with a temperature drop of 7°C every 30 minutes.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention adds 1,5-pentanedithiol, 4-diethylaminobenzaldehyde, an activator (ammonium metatungstate), 2,7-octadienol, etc. These components have good chemical adsorption and physical adsorption properties for nickel in nickel-cobalt ore. Therefore, the obtained mineral processing agent has the characteristics of high separation efficiency, high nickel metal yield and low agent dosage, and is suitable for the application of nickel flotation in nickel-cobalt ore.
[0024] 2. The preparation process of the mineral processing agent of the present invention is simple, reliable and easy to operate. DETAILED DESCRIPTION
[0025] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1, a beneficiation agent for nickel flotation from nickel iron ore, is prepared from the following raw materials in parts by weight: 5-12 parts of 1,5-pentanedithiol, 15-25 parts of sodium carbonate, 20-30 parts of sodium acetate, 20-25 parts of sodium pyrophosphate, 12-20 parts of 2,2-dihydroxymethylbutyric acid, 3-5 parts of quicklime, 40-60 parts of 4-diethylaminobenzaldehyde, 4-5 parts of an activator (ammonium metatungstate), and 20-40 parts of 2,7-octadienol; comprising the following steps:
[0027] ⑴Weigh the raw materials by weight;
[0028] ⑵ Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare an oily solution A with a volume percentage of 30% to 65%;
[0029] ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir and react for 30-40 minutes to obtain solution B;
[0030] (4) Add 4-diethylaminobenzaldehyde, an activator, 2,7-octadienol and sodium acetate to solution B, stir the reaction at a temperature of 35°C to 65°C for 30 to 60 minutes, and then filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 30% to 70%, and the weight percentage of the aqueous solution is 30% to 70%;
[0031] ⑸Evaporate the filtrate to a specific gravity of 2.64-4.37 g / cm 3 After that, cool to 5-30°C and filter the coolant for 45-100 minutes to obtain the product.
[0032] Example 2, according to the ore dressing agent for flotation of nickel from nickel-iron ore and its preparation method described in Example 1, it is made of the following raw materials in parts by weight: 5 of 1,5-pentanedithiol, 15 of sodium carbonate, 20 of sodium acetate, 20 of sodium pyrophosphate, 12 of 2,2-dihydroxymethylbutyric acid, 3 of quicklime, 40 of 4-diethylaminobenzaldehyde, 4 of activator (ammonium metatungstate), and 20 of 2,7-octadienol.
[0033] Example 3, according to Example 1 or 2, a beneficiation agent for flotation of nickel from nickel-iron ore and its preparation method are made from the following raw materials in parts by weight: 12 parts of 1,5-pentanedithiol, 25 parts of sodium carbonate, 30 parts of sodium acetate, 25 parts of sodium pyrophosphate, 20 parts of 2,2-dihydroxymethylbutyric acid, 5 parts of quicklime, 60 parts of 4-diethylaminobenzaldehyde, 5 parts of activator (ammonium metatungstate), and 40 parts of 2,7-octadienol.
[0034] Example 4, according to any one of Examples 1-3, a beneficiation agent for flotation of nickel from nickel-iron ore and a preparation method thereof are prepared from the following raw materials in parts by weight: 9 parts of 1,5-pentanedithiol, 20 parts of sodium carbonate, 25 parts of sodium acetate, 23 parts of sodium pyrophosphate, 16 parts of 2,2-dihydroxymethylbutyric acid, 4 parts of quicklime, 50 parts of 4-diethylaminobenzaldehyde, 4.5 parts of activator (ammonium metatungstate), and 30 parts of 2,7-octadienol.
[0035] Example 5, in the ore dressing agent for flotation of nickel from nickel-iron ore and the preparation method thereof according to any one of Examples 1-4, the activator (ammonium metatungstate) is 4-terpene alcohol.
[0036] Example 6, according to any one of Examples 1-5, in a beneficiation agent for flotation of nickel from nickel-iron ore and a preparation method thereof, the 1,5-pentanedithiol is prepared by the following method: the following raw materials in parts by weight, 1 part of 3-hexyne, 1 part of hydrobromic acid and 2 parts of sodium hydrosulfide are mixed and heated to 400°C.
[0037] Example 7, according to any one of Examples 1-6, in the beneficiation agent for nickel flotation from nickel-iron ore and the preparation method thereof, the stirring reaction in step (3) is carried out for 35 minutes, and the stirring rate is 85 to 130 rpm, preferably 105 rpm.
[0038] Example 8, according to any one of Examples 1-7, a ore dressing agent for flotation of nickel from nickel-iron ore and a preparation method thereof,
[0039] Example 9, according to any one of Examples 1-8, in a beneficiation agent for flotation of nickel from nickel-iron ore and a preparation method thereof, in step (4), the temperature is 50°C, the stirring reaction time is 45 min, and the stirring rate is 35-125 rpm, preferably 80 rpm.
[0040] Example 10, according to any one of Examples 1-9, in a beneficiation agent for flotation of nickel from nickel-iron ore and a preparation method thereof, the cooling method in step (5) adopts gradient cooling, cooling by 5 to 10°C every 30 minutes, preferably cooling by 7°C every 30 minutes.
[0041] Example 11, a beneficiation agent for flotation of nickel from nickel-iron ore, the beneficiation agent is made of the following raw materials: 5 g of 1,5-pentanedithiol, 15 g of sodium carbonate, 20 g of sodium acetate, 20 g of sodium pyrophosphate, 12 g of 2,2-dihydroxymethylbutyric acid, 3 g of quicklime, 40 g of 4-diethylaminobenzaldehyde, 4 g of activator (ammonium metatungstate), and 20 g of 2,7-octadienol.
[0042] The preparation method thereof comprises the following steps:
[0043] ⑴Weigh according to the ratio;
[0044] (2) Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare a 30% by volume oily solution A;
[0045] ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir at 85 rpm for 30 min to obtain solution B;
[0046] (4) Add 4-diethylaminobenzaldehyde, activator (ammonium metatungstate), 2,7-octadienol and sodium acetate to solution B, stir and react at 35°C and 35 rpm for 60 min, and then filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 30% and the weight percentage of the aqueous solution is 70%;
[0047] ⑸Evaporate the filtrate to a specific gravity of 2.64 g / cm 3 Afterwards, the mixture is cooled by gradient cooling, with the temperature decreasing by 5-10°C every 30 minutes to 5°C. The cooling liquid is filtered for 45 minutes to obtain a beneficiation agent for nickel flotation from nickel-cobalt ore.
[0048] The prepared mineral processing agent is named LZY-29 and is used in the flotation of a nickel-cobalt mine in Inner Mongolia. The recovery rate of metallic nickel is shown in Table 1 below:
[0049] Table 1
[0050]
[0051] Example 12, a beneficiation agent for flotation of nickel from nickel-iron ore, the beneficiation agent is made of the following raw materials: 12g of 1,5-pentanedithiol, 25g of sodium carbonate, 30g of sodium acetate, 25g of sodium pyrophosphate, 20g of 2,2-dihydroxymethylbutyric acid, 5g of quicklime, 60g of 4-diethylaminobenzaldehyde, 5g of activator (ammonium metatungstate), and 40g of 2,7-octadienol.
[0052] The preparation method thereof comprises the following steps:
[0053] ⑴Weigh according to the ratio;
[0054] (2) Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare an oily solution A with a volume percentage of 65%;
[0055] ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir at 130 rpm for 40 min to obtain solution B;
[0056] (4) Add 4-diethylaminobenzaldehyde, activator (ammonium metatungstate), 2,7-octadienol and sodium acetate to solution B, stir and react at 65°C and 125 rpm for 30 min, and then filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 70% and the weight percentage of the aqueous solution is 30%;
[0057] ⑸Evaporate the filtrate to a specific gravity of 4.37 g / cm 3 Afterwards, the ore is cooled to 30°C by gradient cooling at a rate of 5-10°C every 30 minutes, and the cooling liquid is filtered for 100 minutes to obtain a beneficiation agent for nickel flotation from nickel-cobalt ore.
[0058] The prepared mineral processing agent is named LZY-29 and is used in the flotation of a nickel-cobalt mine in Qinghai Province. The nickel recovery rate is shown in Table 2 below:
[0059] Table 2
[0060]
[0061] Example 13, a beneficiation agent for flotation of nickel from nickel-iron ore, the beneficiation agent is made of the following raw materials: 10g of 1,5-pentanedithiol, 18g of sodium carbonate, 25g of sodium acetate, 22g of sodium pyrophosphate, 16g of 2,2-dihydroxymethylbutyric acid, 4g of quicklime, 50g of 4-diethylaminobenzaldehyde, 5g of activator (ammonium metatungstate), and 30g of 2,7-octadienol.
[0062] The preparation method thereof comprises the following steps:
[0063] ⑴Weigh according to the ratio;
[0064] (2) Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare an oily solution A with a volume percentage of 45%;
[0065] ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir at 100 rpm for 30 min to obtain solution B;
[0066] (4) Add 4-diethylaminobenzaldehyde, activator (ammonium metatungstate), 2,7-octadienol and sodium acetate to solution B, stir and react at 50°C and 100 rpm for 30 min, and then filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 45% and the weight percentage of the aqueous solution is 55%;
[0067] ⑸Evaporate the filtrate to a specific gravity of 3.58 g / cm 3 Afterwards, the mixture is cooled by gradient cooling, with the temperature decreasing by 5-10°C every 30 minutes to 20°C. The cooling liquid is filtered for 60 minutes to obtain a beneficiation agent for nickel flotation from nickel-cobalt ore.
[0068] The prepared mineral processing agent is named LZY-29 and is used in the flotation of a nickel-cobalt mine in Sichuan Province. The nickel recovery rate is shown in Table 3 below:
[0069] Table 3
[0070]
[0071] Example 14, a beneficiation agent for flotation of nickel from nickel-iron ore, the beneficiation agent is made of the following raw materials: 8 g of 1,5-pentanedithiol, 22 g of sodium carbonate, 26 g of sodium acetate, 23 g of sodium pyrophosphate, 15 g of 2,2-dihydroxymethylbutyric acid, 5 g of quicklime, 46 g of 4-diethylaminobenzaldehyde, 4.5 g of activator (ammonium metatungstate), and 27 g of 2,7-octadienol.
[0072] The preparation method thereof comprises the following steps:
[0073] ⑴Weigh according to the ratio;
[0074] (2) Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare an oily solution A with a volume percentage of 37%;
[0075] ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir at 90 rpm for 35 min to obtain solution B;
[0076] (4) Add 4-diethylaminobenzaldehyde, activator (ammonium metatungstate), 2,7-octadienol and sodium acetate to solution B, stir at 40°C and 80 rpm for 50 min, and filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 52% and the weight percentage of the aqueous solution is 48%;
[0077] ⑸Evaporate the filtrate to a specific gravity of 3.92 g / cm 3 Afterwards, the mixture is cooled by gradient cooling, with the temperature decreasing by 5-10°C every 30 minutes to 10°C. The cooling liquid is filtered for 60 minutes to obtain a beneficiation agent for nickel flotation from nickel-cobalt ore.
[0078] The prepared mineral processing agent was named LZY-29 and was applied to the flotation of a nickel-cobalt mine in the Qilian Mountain area. The nickel recovery rate is shown in Table 4 below:
[0079] Table 4
[0080]
[0081] Example 15 A beneficiation agent for flotation of nickel from nickel-iron ore, the beneficiation agent is made of the following raw materials: 6 g of 1,5-pentanedithiol, 18 g of sodium carbonate, 22 g of sodium acetate, 22 g of sodium pyrophosphate, 17 g of 2,2-dihydroxymethylbutyric acid, 3 g of quicklime, 52 g of 4-diethylaminobenzaldehyde, 5 g of activator (ammonium metatungstate), and 28 g of 2,7-octadienol.
[0082] The preparation method thereof comprises the following steps:
[0083] ⑴Weigh according to the ratio;
[0084] (2) Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare an oily solution A with a volume percentage of 35%;
[0085] ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir at 90 rpm for 35 min to obtain solution B;
[0086] (4) Add 4-diethylaminobenzaldehyde, activator (ammonium metatungstate), 2,7-octadienol and sodium acetate to solution B, stir at 50°C and 90 rpm for 40 min, and filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 50% and the weight percentage of the aqueous solution is 50%;
[0087] ⑸Evaporate the filtrate to a specific gravity of 3.25g / cm 3 Afterwards, the mixture is cooled by gradient cooling, with the temperature decreasing by 5-10°C every 30 minutes to 20°C. The cooling liquid is filtered for 80 minutes to obtain a beneficiation agent for nickel flotation from nickel-cobalt ore.
[0088] The prepared mineral processing agent is named LZY-29 and is used in the flotation of a nickel-cobalt mine in Gansu Province. The recovery rate of metallic nickel is shown in Table 5 below:
[0089] Table 5
[0090]
[0091] The above is only a preferred embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solution and invention concept of the present invention within the scope disclosed by the present invention, which shall fall within the protection scope of the present invention.
Claims
1. A ore dressing agent for flotation of nickel from nickel ferronickel ore, characterized in that: The invention is prepared from the following raw materials in parts by weight: 5-12 parts of 1,5-pentanedithiol, 15-25 parts of sodium carbonate, 20-30 parts of sodium acetate, 20-25 parts of sodium pyrophosphate, 12-20 parts of 2,2-dihydroxymethylbutyric acid, 3-5 parts of quicklime, 40-60 parts of 4-diethylaminobenzaldehyde, 4-5 parts of an activator and 20-40 parts of 2,7-octadienol.
2. The ore dressing agent for nickel flotation from nickel ferronickel ore according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 5 parts of 1,5-pentanedithiol, 15 parts of sodium carbonate, 20 parts of sodium acetate, 20 parts of sodium pyrophosphate, 12 parts of 2,2-dihydroxymethylbutyric acid, 3 parts of quicklime, 40 parts of 4-diethylaminobenzaldehyde, 4 parts of an activator, and 20 parts of 2,7-octadienol.
3. The ore dressing agent for nickel flotation from nickel ferronickel ore according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 12 parts of 1,5-pentanedithiol, 25 parts of sodium carbonate, 30 parts of sodium acetate, 25 parts of sodium pyrophosphate, 20 parts of 2,2-dihydroxymethylbutyric acid, 5 parts of quicklime, 60 parts of 4-diethylaminobenzaldehyde, 5 parts of an activator, and 40 parts of 2,7-octadienol.
4. The ore dressing agent for nickel flotation from nickel ferronickel ore according to claim 1, characterized in that: The invention is prepared from the following raw materials in parts by weight: 9 parts of 1,5-pentanedithiol, 20 parts of sodium carbonate, 25 parts of sodium acetate, 23 parts of sodium pyrophosphate, 16 parts of 2,2-dihydroxymethylbutyric acid, 4 parts of quicklime, 50 parts of 4-diethylaminobenzaldehyde, 4.5 parts of an activator and 30 parts of 2,7-octadienol.
5. The ore dressing agent for flotation of nickel from nickel ferronickel ore according to claim 1, characterized in that: The activator is 4-terpene alcohol.
6. The ore dressing agent for nickel flotation from nickel ferronickel ore according to claim 1, characterized in that: The 1,5-pentanedithiol is prepared by the following method: the following raw materials in parts by weight, 1 part of 3-hexyne, 1 part of hydrobromic acid and 2 parts of sodium hydrosulfide are mixed and heated to 400° C.
7. A method for preparing a nickel ore flotation dressing agent for nickel iron ore, characterized in that: The steps include: ⑴Weigh the raw materials by weight; ⑵ Mix 1,5-pentanedithiol, sodium pyrophosphate and quicklime to prepare an oily solution A with a volume percentage of 30% to 65%; ⑶ Add 2,2-dihydroxymethylbutyric acid and sodium carbonate to solution A, stir and react for 30-40 minutes to obtain solution B; (4) Add 4-diethylaminobenzaldehyde, an activator, 2,7-octadienol and sodium acetate to solution B, stir the reaction at a temperature of 35°C to 65°C for 30 to 60 minutes, and then filter to obtain a filtrate; the filtrate is a mixture of an oily liquid and an aqueous solution, wherein the weight percentage of the oily liquid is 30% to 70%, and the weight percentage of the aqueous solution is 30% to 70%; ⑸Evaporate the filtrate to a specific gravity of 2.64-4.37 g / cm 3 After that, cool to 5-30°C and filter the coolant for 45-100 minutes to obtain the product.
8. The method for preparing a nickel-iron ore flotation nickel dressing agent according to claim 7, characterized in that: In the step (3), the reaction was stirred for 35 minutes at a stirring speed of 105 rpm.
9. The method for preparing a nickel-iron ore flotation nickel dressing agent according to claim 1, characterized in that: In the step (4), the temperature is 50° C., the stirring reaction time is 45 min, and the stirring rate is 80 rpm.
10. The method for preparing a nickel-iron ore flotation nickel dressing agent according to claim 1, characterized in that: In the step (5), the cooling method adopts gradient cooling, with a temperature drop of 7° C. every 30 minutes.
Citation Information
Patent Citations
Combined inhibitor used for flotation of low-grade nickel ore with high content of sliding magnesium rock
CN102716812A
Beneficiation reagent for copper sulfide ore
CN103464298A
Beneficiation reagent for nickel flotation of nickel-cobalt ore and preparation method of beneficiation reagent
CN117380399A
Method for processing low-grade laterite nickel ore and beneficiation method therefor
WO2017185946A1