Compound spraying method

Through the duplex spraying method, the combination of acid degreasing agent and specific raw materials is used to solve the problem of insufficient bonding of aluminum alloy profile coating and matrix, and efficient oxidation and wear resistance are achieved, extending service life and reducing costs.

CN118976675APending Publication Date: 2024-11-19SHANXI LIGONG MECHANICAL & ELECTRICAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411341539.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing spraying process, the oxidation of aluminum alloy profiles and insufficient bonding of coatings and substrates lead to a shortened service life and an increase in cost, and thermal spraying methods will affect the performance of the substrate.

Method used

Using the duplex spraying method, including substrate pretreatment, spray primer layer, topcoat layer, curing treatment and hood coating, the combination of acid degreasing agents and specific raw materials improves the binding force and oxidation resistance of the coating and the substrate to avoid high temperatures deal with.

Benefits of technology

It improves the bonding strength and oxidation resistance of the coating to the substrate, extends the service life, reduces costs, and improves the wear and corrosion resistance of the coating, with a smooth surface and strong adhesion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a compound spraying method which comprises the following steps: (1) substrate pretreatment: performing rust removal, degreasing, oil removal and dirt removal treatment on a substrate, washing with water, drying and standing; (2) spraying prime paint; spraying a primer layer with the thickness of 5-10 microns on the pretreated matrix; (3) spraying a finish paint layer; spraying a finish paint layer with the thickness of 20-25 mu m on the substrate sprayed with the prime paint; (4) curing treatment; carrying out curing treatment on the base body sprayed with the finish paint; and (5) spraying a finishing paint layer on the cured substrate. According to the compound spraying method, on the premise that the temperature is not too high, the bonding performance between the coating and the base body is improved, the bonding strength is improved, excellent wear resistance and corrosion resistance are achieved, and the sprayed base body is smooth in surface, low in oil stain adhesive force and free of fingerprints.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of spraying technology, and more specifically to a compound spraying method. Background Art

[0002] At present, aluminum alloy is the most widely used type of nonferrous metal structural material in industry, and has been widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. In order to prevent the oxidation of aluminum alloy profiles and plates and extend the service life of aluminum alloy profiles, it is necessary to spray the surface of aluminum alloy materials. However, since the degreasing and pickling are simply performed in the pre-spraying process, the surface of aluminum alloy cannot have strong adhesion. When used, it is eroded by pollution such as air and acid rain, and the penetration of ultraviolet rays shortens the service life of aluminum and increases the cost of use.

[0003] The existing thermal spray coating is generally bonded to the substrate by mechanical bonding. The coating structure is a typical layered structure with obvious directional properties, so interlayer failure or coating peeling is prone to occur. In order to improve the bonding strength, the substrate surface is often treated by surface cladding or spray welding to achieve a metallurgical bonding state between the coating and the substrate. However, this method will cause the substrate to overheat (usually above 1000°C) and will also have a significant impact on the performance of the surface layer and the substrate.

[0004] Therefore, how to solve the defects of high cost and high temperature in the spraying process, which affect the bonding between the substrate and the coating, is an urgent problem that technicians in this field need to solve. Summary of the invention

[0005] In view of this, the present invention provides a compound spraying method, the purpose of which is to enhance the bonding between the spray layer and the substrate, improve the bonding strength and enhance the antioxidant ability.

[0006] To achieve the above object, the present invention provides a compound spraying method, comprising the following steps:

[0007] (1) Substrate pretreatment: rust removal, degreasing, deoiling and decontamination treatment of the substrate, washing with water, drying and standing;

[0008] (2) spraying primer: spraying a primer layer of 5-10 μm on the pretreated substrate;

[0009] (3) Spraying topcoat: spraying a 20-25 μm topcoat layer on the substrate after spraying the basecoat.

[0010] (4) Curing treatment: Curing treatment is performed on the substrate after spraying the topcoat.

[0011] (5) Spray a finishing paint layer on the cured substrate.

[0012] The beneficial effects of the above technical scheme are as follows: the present invention is treated with an acidic degreasing agent before spraying, which increases the bonding force and anti-oxidation ability of the coating and the aluminum alloy surface, and is conducive to extending the service life of the base paint layer; the primer layer improves the anti-penetration ability of the coating, enhances the protection of the base, stabilizes the base surface layer, strengthens the adhesion between the topcoat layer and the base surface, and ensures the uniform color of the topcoat layer; the topcoat layer protects the base surface from the erosion of the external environment atmosphere, acid rain, and pollution, prevents ultraviolet rays from penetrating, and greatly enhances the anti-aging ability; and the finishing varnish coating further enhances the aesthetics and color of the base surface and protects the topcoat layer. The curing treatment enhances the adhesion between the coatings.

[0013] Preferably, the rust removal, degreasing, deoiling and decontamination treatment in step (1) is to place the substrate in an acidic degreasing agent solution, immerse it for 3 to 4 minutes, control the temperature to 20 to 50°C, then rinse it with clean water for 3 to 5 minutes, and then put the substrate into an oven for drying at a temperature of 150 to 200°C for 5 to 10 minutes.

[0014] Preferably, the acidic degreasing agent comprises the following raw material components in parts by weight: 30-50 parts of 97% sulfuric acid, 5-10 parts of citric acid, 3-8 parts of ammonium bifluoride, 1-3 parts of sodium nitrate, 0.5-2 parts of ferric sulfate, 0.5-2 parts of trichloroethylene, 0.05-0.4 parts of fluorocarbon solvent; and 3-10 parts of surfactant.

[0015] Preferably, the raw material components and weight proportions of the primer layer in step (2) are as follows: 8-10 parts of ethyl acetate, 20-40 parts of thermoplastic acrylic resin, 3-5 parts of diethylene glycol ethyl ether, 10-15 parts of magnesium powder, 0.5-3 parts of propylene glycol monopropyl ether, 0.5-2 parts of diethylene glycol ethyl ether, and 0.05-0.5 parts of polydimethylsiloxane.

[0016] Preferably, the topcoat layer in step (3) comprises the following raw material components in parts by weight: 10-15 parts of polyurethane, 20-30 parts of toluene, 8-12 parts of butyl acetate, 1.5-5.5 parts of nano-silicon dioxide, 2.5-6.5 parts of nano-silicon carbide, and 0.5-1.5 parts of polydimethylsiloxane.

[0017] Preferably, in step (4), the curing agent is isophorone diamine, diaminodiphenylmethane or benzylenediamine trimer, the ratio of the curing agent to the topcoat is 1:40-70, the curing time is 20-30 minutes, and the curing temperature is 150°C.

[0018] Preferably, the thickness of the finishing paint layer is 5-10 μm; the raw material of the finishing paint layer is polyvinylidene fluoride resin.

[0019] It can be seen from the above technical solution that compared with the prior art, the compound spraying method disclosed in the present invention improves the bonding between the coating and the substrate without making the temperature too high, thereby enhancing the bonding strength and having excellent wear resistance and corrosion resistance. The surface of the substrate after spraying is smooth, the oil adhesion is low, and no fingerprints are left. DETAILED DESCRIPTION

[0020] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] A composite spraying method comprises the following steps:

[0023] The following raw materials are weighed in parts by weight to prepare an acidic degreasing agent: 30 parts of 97% sulfuric acid, 5 parts of citric acid, 3 parts of ammonium bifluoride, 1 part of sodium nitrate, 0.5 parts of ferric sulfate, 0.5 parts of trichloroethylene, 0.05 parts of a fluorocarbon solvent; 3 parts of a surfactant;

[0024] The following raw materials were weighed in parts by weight to prepare a primer spray paint: 8 parts of ethyl acetate, 20 parts of thermoplastic acrylic resin, 3 parts of diethylene glycol ethyl ether, 10 parts of magnesium powder, 0.5 parts of propylene glycol monopropyl ether, and 0.05 parts of polydimethylsiloxane;

[0025] The raw materials are weighed according to the following weight parts to prepare the topcoat spray paint: 10 parts of polyurethane, 20 parts of toluene, 8 parts of butyl acetate, 1.5 parts of nano-silicon dioxide, 2.5 parts of nano-silicon carbide, and 0.5 parts of polydimethylsiloxane;

[0026] (1) placing the substrate in the prepared acidic solution, immersing for 3 minutes at a temperature of 20° C., then washing with clean water for 3 minutes, and placing in a 150° C. oven for 5 minutes to complete substrate pretreatment;

[0027] (2) spraying a 5 μm primer layer on the pretreated substrate;

[0028] (3) spraying a 20 μm topcoat layer on the substrate after spraying the primer;

[0029] (4) Curing the substrate after spraying the topcoat layer for 20 minutes at a ratio of primer to curing agent of 40:1;

[0030] (5) spraying a 5 μm topcoat coating layer on the cured substrate;

[0031] The raw material of the finishing paint layer is polyvinylidene fluoride resin.

[0032] Example 2

[0033] A composite spraying method comprises the following steps:

[0034] The following raw materials are weighed in parts by weight to prepare an acidic degreasing agent: 40 parts of 97% sulfuric acid, 7 parts of citric acid, 5 parts of ammonium bifluoride, 2 parts of sodium nitrate, 1 part of ferric sulfate, 1.5 parts of trichloroethylene, 0.2 parts of a fluorocarbon solvent, and 6 parts of a surfactant;

[0035] The raw materials were weighed according to the following weight parts to prepare the primer spray paint: 9 parts of ethyl acetate, 30 parts of thermoplastic acrylic resin, 4 parts of diethylene glycol ethyl ether, 13 parts of magnesium powder, 2 parts of propylene glycol monopropyl ether, and 0.3 parts of polydimethylsiloxane;

[0036] The raw materials are weighed according to the following weight parts to prepare the topcoat spray paint: 13 parts of polyurethane, 25 parts of toluene, 10 parts of butyl acetate, 3 parts of nano silicon dioxide, 4 parts of nano silicon carbide, and 1 part of polydimethylsiloxane;

[0037] (1) placing the substrate in the prepared acidic solution, immersing for 3 minutes at a temperature of 40° C., then washing with clean water for 4 minutes, and placing in an oven at 170° C. for 7 minutes to complete substrate pretreatment;

[0038] (2) spraying a 7 μm primer layer on the pretreated substrate;

[0039] (3) spraying a 23 μm topcoat layer on the substrate after spraying the primer;

[0040] (4) Curing the substrate after spraying the topcoat layer for 25 minutes at a ratio of primer to curing agent of 50:1;

[0041] (5) spraying a 7 μm topcoat coating layer on the cured substrate;

[0042] The raw material of the finishing paint layer is polyvinylidene fluoride resin.

[0043] Example 3

[0044] A composite spraying method comprises the following steps:

[0045] The following raw materials are weighed in parts by weight to prepare an acidic degreasing agent: 50 parts of 97% sulfuric acid, 10 parts of citric acid, 8 parts of ammonium bifluoride, 3 parts of sodium nitrate, 2 parts of ferric sulfate, 2 parts of trichloroethylene, 0.4 parts of a fluorocarbon solvent, and 10 parts of a surfactant;

[0046] The following raw materials were weighed in parts by weight to prepare a primer spray paint: 10 parts of ethyl acetate, 40 parts of thermoplastic acrylic resin, 5 parts of diethylene glycol ethyl ether, 15 parts of magnesium powder, 3 parts of propylene glycol monopropyl ether, and 0.5 parts of polydimethylsiloxane;

[0047] The raw materials are weighed according to the following weight parts to prepare the topcoat spray paint: 15 parts of polyurethane, 30 parts of toluene, 12 parts of butyl acetate, 5.5 parts of nano silicon dioxide, 6.5 parts of nano silicon carbide, and 1.5 parts of polydimethylsiloxane;

[0048] (1) placing the substrate in the prepared acidic solution, immersing for 4 minutes at a temperature of 50° C., then washing with clean water for 5 minutes, and placing in a 200° C. oven for 10 minutes to complete substrate pretreatment;

[0049] (2) spraying a 10 μm primer layer on the pretreated substrate;

[0050] (3) spraying a 25 μm topcoat layer on the substrate after spraying the primer;

[0051] (4) Curing the substrate after spraying the topcoat layer for 30 minutes at a ratio of primer to curing agent of 70:1;

[0052] (5) spraying a 10 μm topcoat coating layer on the cured substrate;

[0053] The raw material of the finishing paint layer is polyvinylidene fluoride resin.

[0054] The spray-coated substrates obtained in Examples 1-3 were tested to have a friction coefficient of less than 0.1, and a smooth surface with a matte color. The test results of the hardness (GB / T6739-1996), wear resistance (GB / T1768-2006), and corrosion resistance (GB / T20854-2007) of the coating are shown in Table 1 below.

[0055] Table 1 Test results

[0056] Serial number Wear resistance Corrosion resistance Hardness (HRC) Example 1 94 2961h 28.4 Example 2 97 2994h 28.7 Example 3 98 3011h 28.9

[0057] Therefore, the compound spraying method disclosed in the present invention can improve the bonding between the coating and the substrate without making the temperature too high, enhance the bonding strength, and have excellent wear resistance and corrosion resistance. The surface of the substrate after spraying is smooth, the oil adhesion is low, and no fingerprints will be left.

[0058] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0059] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A compound spraying method, characterized in that: The following steps are involved: (1) Substrate pretreatment: rust removal, degreasing, deoiling and decontamination treatment of the substrate, washing with water, drying and standing; (2) spraying primer: spraying a primer layer of 5-10 μm on the pretreated substrate; (3) Spraying a topcoat layer; spraying a 20-25 μm topcoat layer on the substrate after spraying the basecoat; (4) Curing treatment: Curing the substrate after spraying the topcoat; (5) Spray a finishing paint layer on the cured substrate.

2. A compound spraying method according to claim 1, characterized in that: The rust removal, degreasing, deoiling and decontamination treatment in step (1) is to place the substrate in an acidic degreasing agent solution, immerse it for 3 to 4 minutes, control the temperature to be 20 to 50° C., then rinse it with clean water for 3 to 5 minutes, and then put the substrate into an oven for drying at a temperature of 150 to 200° C. for 5 to 10 minutes.

3. A compound spraying method according to claim 2, characterized in that: The acidic degreasing agent comprises the following raw material components in parts by weight: 30-50 parts of 97% sulfuric acid, 5-10 parts of citric acid, 3-8 parts of ammonium bifluoride, 1-3 parts of sodium nitrate, 0.5-2 parts of ferric sulfate, 0.5-2 parts of trichloroethylene, 0.05-0.4 parts of fluorocarbon solvent; and 3-10 parts of surfactant.

4. A compound spraying method according to claim 1, characterized in that: The raw material components and weight proportions of the primer layer in step (2) are as follows: 8-10 parts of ethyl acetate, 20-40 parts of thermoplastic acrylic resin, 3-5 parts of diethylene glycol ethyl ether, 10-15 parts of magnesium powder, 0.5-3 parts of propylene glycol monopropyl ether, and 0.05-0.5 parts of polydimethylsiloxane.

5. A compound spraying method according to claim 1, characterized in that: The topcoat layer in step (3) comprises the following raw material components in parts by weight: 10-15 parts of polyurethane, 20-30 parts of toluene, 8-12 parts of butyl acetate, 1.5-5.5 parts of nano-silicon dioxide, 2.5-6.5 parts of nano-silicon carbide, and 0.5-1.5 parts of polydimethylsiloxane.

6. A compound spraying method according to claim 1, characterized in that: In the step (4), the curing agent is isophorone diamine, diaminodiphenylmethane or benzylenediamine trimer, the ratio of the curing agent to the topcoat is 1:40-70, and the curing time is 20-30 minutes.

7. A compound spraying method according to claim 1, characterized in that: The thickness of the finishing paint layer is 5-10 μm; The raw material of the finishing paint layer is polyvinylidene fluoride resin.