Carrier cleaning method

By removing the deposited layer on the vehicle and forming a fixed layer, the problems of short service life and high cost of the vehicle during the growth of the silicon carbide epitaxial sheet are solved, the cleaning and repair of the vehicle are achieved, and the quality and yield of the epitaxial sheet are improved. .

CN118976753APending Publication Date: 2024-11-19TIANJIN HUANYAO NEW MATERIAL TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411047399.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the growth of silicon carbide epitaxial sheets, deposits on the carrier will cause an increase in the doping concentration of the substrate edge, affecting the uniformity of the epitaxial layer, resulting in a short service life and high cost of the carrier.

Method used

By removing the deposited layer and performing heat treatment and surface treatment on the vehicle, a fixed layer is formed to cover the residual silicon carbide particles, and the thickness ratio of the deposited layer and the fixed layer is controlled to be within the range of 18≤H1/H2≤29, to achieve vehicle cleaning and repair.

Benefits of technology

It extends the service life of the vehicle, improves the quality and yield of the epitaxial sheet, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976753A_ABST
    Figure CN118976753A_ABST
Patent Text Reader

Abstract

The invention discloses a carrier cleaning method, and relates to the technical field of semiconductor manufacturing. The carrier cleaning method is used for cleaning a carrier after an epitaxial reaction, the carrier is coated with a coating, one side of the coating is provided with a deposition layer, and the cleaning method comprises the steps that at least part of the deposition layer is removed, and the carrier coated with the coating is obtained; and carrying out heat treatment and surface treatment on the carrier coated with the coating so as to complete cleaning of the carrier. The carrier after the epitaxial reaction is subjected to cleaning treatment such as deposition layer removal, heating treatment and surface treatment, cleaning of the carrier can be achieved, and meanwhile the service life of the carrier can be prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for cleaning a carrier. Background Art

[0002] Silicon carbide (SiC) material is a wide bandgap compound semiconductor material with characteristics such as high breakdown field strength, high thermal conductivity and high electron saturation drift rate. SiC epitaxial wafers are usually grown epitaxially in an epitaxial cavity using chemical vapor deposition. However, while the epitaxial layer is formed on the surface of the SiC substrate, a deposit is also formed on the epitaxial carrier. As the carrier continues to be used, the elements in the deposit will gradually overflow and diffuse to the edge of the silicon carbide substrate, resulting in an increase in the edge concentration of the silicon carbide epitaxial layer, thereby causing the concentration uniformity of the silicon carbide epitaxial wafer to deteriorate. On the other hand, the carrier used for epitaxial growth will be scrapped due to the formation of a certain thickness of SiC deposits on the carrier, which will also cause the epitaxial concentration uniformity of the carrier to deteriorate. Therefore, it has the disadvantages of short service life and high cost. Summary of the invention

[0003] The purpose of the present application is to provide a method for cleaning a carrier, which can achieve cleaning of the carrier and also increase the service life of the carrier.

[0004] The embodiment of the present application provides a carrier cleaning method for cleaning a carrier after an epitaxial reaction, wherein the carrier is covered with a coating, and a deposition layer is provided on one side of the coating. The cleaning method comprises:

[0005] removing at least a portion of the deposited layer to obtain a carrier covered with a coating;

[0006] The carrier covered with the coating is subjected to heat treatment and surface treatment to complete the cleaning of the carrier.

[0007] In some embodiments, the surface treatment method comprises:

[0008] Placing the carrier in the reaction chamber;

[0009] Allowing a carbon source and a silicon source to flow into the reaction chamber to form a fixed layer on the carrier after the heat treatment;

[0010] The carbon source includes carbon element, the silicon source includes silicon element, and the ratio of the number of atoms of the carbon element to the number of atoms of the silicon element is in the range of 0.6-1.

[0011] In some embodiments, the deposited layer has a first thickness H1, measured in μm, and the fixed layer has a second thickness H2, measured in μm, satisfying: 18≤H1 / H2≤29.

[0012] In some embodiments, the first thickness H1 ranges from 180 to 200 μm.

[0013] In some embodiments, the second thickness H2 is in the range of 7 to 10 μm.

[0014] In some embodiments, the flow rate of the carbon source is in the range of 114 to 150 sccm.

[0015] In some embodiments, the silicon source flow rate is 300 sccm.

[0016] In some embodiments, the carbon source is selected from at least one of ethylene, acetylene, methane, and propane.

[0017] In some embodiments, the silicon source is selected from at least one of silane or silane derivatives.

[0018] In some embodiments, the temperature of the reaction chamber is 1580-1600° C., and the pressure of the reaction chamber is 90-110 mbar.

[0019] In some embodiments, the time for forming the fixed layer is 480 to 680 seconds.

[0020] In some embodiments, the heat treatment temperature is 1580-1640° C., and the heat treatment time is 30-60 min.

[0021] In some embodiments, the heat treatment device is selected from an epitaxial furnace.

[0022] In some embodiments, the heat treatment device is selected from any one of a hot-wall horizontal epitaxial furnace, a warm-wall planetary epitaxial furnace, and a quasi-hot-wall vertical epitaxial furnace.

[0023] In some embodiments, the method of removing at least a portion of the deposited layer comprises:

[0024] The deposited layer is polished to remove at least a portion of the deposited layer.

[0025] In some embodiments, the epitaxial carrier comprises a graphite ring.

[0026] In some embodiments, the coating is made of silicon carbide.

[0027] In some embodiments, the carrier cleaning process is performed 1 to 4 times.

[0028] The beneficial effects of this application are:

[0029] The present application provides a carrier cleaning method for cleaning a carrier after an epitaxial reaction, wherein the carrier is covered with a coating, and a deposition layer is provided on one side of the coating. The cleaning method comprises: removing at least part of the deposition layer to obtain a carrier covered with the coating; performing heat treatment and surface treatment on the carrier covered with the coating to complete the cleaning of the carrier. The present application can clean the carrier by performing cleaning treatments such as removal of the deposition layer, heat treatment, and surface treatment on the carrier after an epitaxial reaction, and can also improve the service life of the carrier. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A flow chart of a cleaning method for a carrier provided in an embodiment of the present application;

[0031] Figure 2 It is a schematic diagram of the structure of a graphite ring;

[0032] Figure 3 A surface defect characterization diagram of a silicon carbide epitaxial wafer provided in Example 1 of the present application;

[0033] Figure 4 This is a surface defect characterization diagram of the silicon carbide epitaxial wafer provided for Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0034] The technical solution of the present application will be described clearly and completely below in conjunction with the embodiments and drawings of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application. The various embodiments of the present application may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity, and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values ​​within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which are applicable regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range.

[0035] See also Figure 1 The embodiment of the present application provides a carrier cleaning method for cleaning a carrier after an epitaxial reaction, wherein the carrier is covered with a coating, and a deposition layer is provided on one side of the coating. The cleaning method comprises:

[0036] S1: removing at least part of the deposited layer to obtain a carrier covered with a coating;

[0037] S2: performing heat treatment and surface treatment on the carrier covered with the coating to complete the cleaning of the carrier;

[0038] It is understandable that during the epitaxial growth of silicon carbide, the substrate is usually placed on a carrier in the epitaxial reaction chamber, and raw materials for forming the silicon carbide epitaxial layer are introduced into the reaction chamber to achieve epitaxial growth of the silicon carbide epitaxial layer on the substrate. However, at the same time, the raw materials for forming the silicon carbide epitaxial layer will also be deposited on the surface of the carrier to form a deposition layer. When the thickness of the deposition layer is too thick, it will cause the doping concentration at the edge of the substrate close to the carrier to increase, and as the carrier rotates during the epitaxial process, the silicon carbide particles on the carrier with an excessively thick deposition layer will fall to the surface of the epitaxial wafer. Continuing to use the carrier will increase the surface defects of the processed epitaxial wafer and make the doping concentration uniform. The properties of the epitaxial wafer will deteriorate, thereby reducing the quality of the epitaxial wafer and ultimately affecting the product yield; when removing the deposited layer, a number of silicon carbide particles will be formed on the surface of the carrier, which are not easy to observe and remove, and these particles may enter the epitaxial wafer during the epitaxial reaction, thereby affecting the quality of the epitaxial wafer and ultimately affecting the product yield; the present application first removes the deposited layer deposited on the carrier, and then performs heat treatment and surface treatment on the carrier after the deposited layer is removed, so as to repair the carrier after the deposited layer is removed, and can cover and fix the silicon carbide particles remaining when the deposited layer is removed, thereby avoiding the influence of the silicon carbide particles on the quality of the epitaxial wafer when the cleaned carrier is used again.

[0039] In some embodiments, the method of surface treatment comprises:

[0040] placing the carrier in the reaction chamber;

[0041] A carbon source and a silicon source are introduced into the reaction chamber to form a fixed layer on the carrier after the heat treatment;

[0042] The carbon source includes carbon, the silicon source includes silicon, and the ratio of the number of atoms of carbon to silicon is in the range of 0.6 to 1. Specifically, the ratio of the number of atoms of carbon to silicon can be any one of 0.6, 0.7, 0.8, 0.9, 1, or a range consisting of any two values.

[0043] It can be understood that the present application forms a fixed layer on the carrier after heat treatment, and the fixed layer can cover and fix the silicon carbide particles remaining when the deposited layer is removed, and by further controlling the C / Si ratio during the formation of the fixed layer, a dense fixed layer can be formed to prevent the residual silicon carbide particles when the deposited layer is removed from passing through the fixed layer at high temperature and overflowing to the surface of the fixed layer, thereby reducing the quality of the epitaxial wafer and ultimately affecting the product yield.

[0044] In some embodiments, the deposited layer has a first thickness H1, in μm, and the fixed layer has a second thickness H2, in μm, satisfying: 18≤H1 / H2≤29. Specifically, the value of H1 / H2 can be any one of 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or a range consisting of any two values.

[0045] It is understandable that whenever the thickness of the deposited layer reaches 180-200 μm, the carrier needs to be cleaned, and the cleaned carrier continues to be used for epitaxial growth; therefore, when the cleaned carrier is used for epitaxial reaction again and the thickness of the deposited layer reaches 180-200 μm again, the carrier needs to be cleaned a second time. At this time, the fixed layer formed during the first cleaning will also affect the life of the carrier. Therefore, if the thickness of the fixed layer formed during cleaning is too thick, the service life of the carrier will be reduced; when the thickness of the fixed layer is too thin, the fixed layer cannot cover and fix the silicon carbide particles remaining when the deposited layer is removed. ; When the thickness of the deposited layer is too thick, if the deposited layer is not removed and the carrier is continued to be used, the surface defects of the processed epitaxial wafer will increase and the concentration uniformity will deteriorate, thereby reducing the quality of the epitaxial wafer and ultimately affecting the product yield; when the thickness of the deposited layer is too thin, continuing to use the carrier will have a negligible impact on the processed epitaxial wafer. In addition, if the deposited layer is too thin, cleaning the carrier will also increase the epitaxial cost. The present application controls the thickness between the deposited layer and the fixed layer to satisfy 18≤H1 / H2≤29, thereby improving the cleaning effect of the carrier and increasing the service life of the carrier, thereby reducing production costs.

[0046] In some embodiments, the deposited layer has a first thickness H1 in μm, and the first thickness H1 ranges from 180 to 200 μm. Specifically, the first thickness H1 can be any one of 180 μm, 185 μm, 190 μm, 195 μm, and 200 μm, or a range consisting of any two values.

[0047] It is understandable that when the thickness of the deposited layer is too thick, if the carrier continues to be used, the surface defects of the processed epitaxial wafer will increase and the concentration uniformity will deteriorate, thereby reducing the quality of the epitaxial wafer and ultimately affecting the product yield; when the thickness of the deposited layer is too thin, continuing to use the carrier will have a negligible impact on the processed epitaxial wafer. If the thickness of the deposited layer is too thin, cleaning the carrier will increase the epitaxial cost. Therefore, the present application controls the thickness of the deposited layer to 180~200μm, which can achieve the cleaning of the carrier and increase the service life of the carrier.

[0048] In some embodiments, the fixed layer has a second thickness H2, in μm, ranging from 7 to 10 μm. Specifically, the second thickness H2 can be any one of 7 μm, 8 μm, 9 μm, and 10 μm, or a range consisting of any two values.

[0049] It can be understood that whenever the thickness of the deposited layer reaches 180-200μm, the carrier needs to be cleaned, and the cleaned carrier continues to be used for epitaxial growth. Therefore, when the cleaned carrier is used for epitaxial reaction again and the thickness of the deposited layer reaches 180-200μm again, the carrier needs to be cleaned for the second time. At this time, the fixed layer formed during the first cleaning will also affect the life of the carrier. Therefore, if the thickness of the fixed layer formed during cleaning is too thick, the service life of the carrier will be reduced; when the thickness of the fixed layer is too thin, the fixed layer cannot cover and fix the silicon carbide particles remaining when the deposited layer is removed, which will increase the surface defects of the processed epitaxial wafer and deteriorate the concentration uniformity, thereby reducing the quality of the epitaxial wafer and ultimately affecting the product yield. Therefore, the present application controls the thickness of the fixed layer to 7-10μm, which can achieve the cleaning of the carrier and improve the service life of the carrier.

[0050] In some embodiments, the carbon source flow rate ranges from 114 to 150 sccm. Specifically, the carbon source flow rate can be any one of 114 sccm, 120 sccm, 125 sccm, 130 sccm, 135 sccm, 140 sccm, 145 sccm, and 150 sccm, or a range consisting of any two of the values.

[0051] In some embodiments, the silicon source flow rate is 300 seem.

[0052] It can be understood that the present application controls the carbon source flow rate and the silicon source flow rate, thereby controlling the ratio of the number of atoms of carbon and silicon elements (C / Si ratio) in the fixed layer formation process within the range of 0.6 to 1 to meet the requirements for the formation of the fixed layer.

[0053] In some embodiments, the carbon source is selected from at least one of ethylene, acetylene, methane, and propane.

[0054] In some embodiments, the silicon source is selected from at least one of silane or silane derivatives.

[0055] In some embodiments, the silane derivative is selected from at least one of trichlorosilane, tetrachlorosilane, and dichlorosilane.

[0056] In some embodiments, the temperature of the reaction chamber is 1580-1600°C, and the pressure of the reaction chamber is 90-110 mbar. Specifically, the temperature of the reaction chamber can be any one of 1580°C, 1585°C, 1590°C, 1595°C, and 1600°C, or a range consisting of any two values; specifically, the pressure of the reaction chamber can be any one of 90 mbar, 95 mbar, 100 mbar, 105 mbar, and 110 mbar, or a range consisting of any two values.

[0057] It is understandable that when forming the fixed layer, the temperature of the reaction chamber is controlled to be 1580-1600° C. and the pressure of the reaction chamber is controlled to be 90-110 mbar to meet the formation requirements of the fixed layer.

[0058] In some embodiments, the time for forming the fixed layer is 480 to 680 seconds. Specifically, the time for forming the fixed layer can be any one of 480 seconds, 530 seconds, 580 seconds, 630 seconds, and 680 seconds, or a range consisting of any two of the values.

[0059] It can be understood that, in the present application, by controlling the formation time of the fixed layer to be 480 to 680 seconds, the thickness of the formed fixed layer can be controlled to meet the requirement of the thickness of the fixed layer.

[0060] In some embodiments, the heat treatment may be in the form of baking.

[0061] In some embodiments, the heat treatment temperature is 1580-1640°C, and the heat treatment time is 30-60 min. Specifically, the heat treatment temperature can be any one of 1580°C, 1590°C, 1600°C, 1610°C, 1620°C, 1630°C, and 1640°C, or a range consisting of any two values; the heat treatment time can be any one of 30 min, 40 min, 50 min, and 60 min, or a range consisting of any two values.

[0062] It is understandable that some silicon carbide particles remain on the carrier when the deposited layer is removed. Through high-temperature baking, the silicon carbide particles remaining on the carrier can be melted and fixed on the graphite ring to prevent these particles from entering the epitaxial wafer during the epitaxial reaction, thereby affecting the quality of the epitaxial wafer and ultimately affecting the product yield.

[0063] In some embodiments, the heat treatment apparatus is selected from an epitaxial furnace.

[0064] In some embodiments, the heat treatment device is selected from any one of a hot-wall horizontal epitaxial furnace, a warm-wall planetary epitaxial furnace, and a quasi-hot-wall vertical epitaxial furnace.

[0065] It is to be understood that the heat treated device may be an epitaxially grown device.

[0066] In some embodiments, a method of removing at least a portion of a deposited layer includes:

[0067] The deposited layer is polished to remove at least a portion of the deposited layer.

[0068] It can be understood that the present application removes the deposited layer by grinding and polishing. Specifically, the deposited layer is removed by mechanical grinding, which can prevent irreversible damage to the carrier and the coating on the surface of the carrier.

[0069] See also Figure 2 In some embodiments, the epitaxial carrier includes a graphite ring.

[0070] It can be understood that the carrier cleaning method provided in the present application can clean the graphite ring epitaxial carrier.

[0071] In some embodiments, the material of the coating is selected from silicon carbide.

[0072] It can be understood that by forming a silicon carbide coating on the surface of the carrier, the smoothness and thickness uniformity of the carrier surface can be improved.

[0073] In some embodiments, the deposited layer includes a deposited silicon carbide layer formed by epitaxial reactive deposition.

[0074] It is understandable that whenever the thickness of the deposited layer reaches 180-200 μm, the carrier needs to be cleaned, and the cleaned carrier continues to be used for epitaxial growth; therefore, when the cleaned carrier is used again for epitaxial reaction and the thickness of the deposited layer reaches 180-200 μm again, the carrier needs to be cleaned a second time, so when the carrier is used for epitaxial reaction for the first time, the deposited layer only includes the silicon carbide deposited layer deposited on the carrier by the epitaxial reaction.

[0075] In some embodiments, the number of times the carrier is cleaned is 1 to 4. Specifically, the number of times the carrier is cleaned can be any one of 1, 2, 3, and 4 times, or a range consisting of any two values.

[0076] It is understandable that when the carrier is cleaned more than 4 times, the surface defects of the carrier increase. If the carrier continues to be used, the surface defects of the processed epitaxial wafers will increase and the concentration uniformity will deteriorate, thereby reducing the quality of the epitaxial wafers and ultimately affecting the product yield.

[0077] In some embodiments, the thickness of the epitaxial wafer is measured using a Fourier transform infrared spectrometer.

[0078] In some embodiments, the thickness of the deposited layer is estimated by accumulating the thickness of the epitaxially grown epitaxial wafer.

[0079] In some embodiments, the thickness of the fixed layer is determined by the growth rate and growth time, wherein the C / Si ratio, reaction chamber temperature and pressure, and source gas flow rate all affect the growth rate.

[0080] In some embodiments, the temperature, pressure and epitaxial growth time of the reaction chamber are controlled by setting the temperature, pressure and epitaxial growth time of the epitaxial device.

[0081] In some embodiments, the flow rate control method of the carbon source and the silicon source is:

[0082] For gas, the gas flow rate is directly controlled by the mass flow meter; for liquid, the flow rate of the corresponding liquid is controlled by controlling the carrier gas flow rate.

[0083] The present application will be described below through specific embodiments.

[0084] Example 1

[0085] S11: providing a graphite ring after a silicon carbide epitaxial reaction, the graphite ring having been cleaned 0 times, having a silicon carbide coating and a silicon carbide deposition layer deposited during the epitaxial reaction, the thickness of the silicon carbide deposition layer being 200 μm;

[0086] S12: removing the silicon carbide deposited layer by mechanical grinding and polishing to obtain a graphite ring covered with a silicon carbide coating;

[0087] S13: baking the graphite ring covered with the silicon carbide coating at 1600° C. for 45 min;

[0088] S14: placing the baked graphite ring in the reaction chamber;

[0089] S15: The temperature of the reaction chamber is regulated to 1580°C and the pressure is 100 mbar, and ethylene and trichlorosilane are introduced into the reaction chamber to grow a first fixed layer on the baked graphite ring; wherein the flow rate of ethylene is 120 sccm, the flow rate of trichlorosilane is 300, the C / Si ratio in the fixed layer is 0.8, the temperature of the reaction chamber is 1580°C, the pressure of the reaction chamber is 100 mbar, the growth time of the fixed layer is 580 s, the thickness of the first fixed layer is 8 μm, and the first cleaning of the graphite ring is completed.

[0090] Example 2

[0091] S11: providing a graphite ring after a silicon carbide epitaxial reaction, wherein the graphite ring participating in the silicon carbide epitaxial reaction has been cleaned once, and the graphite ring includes a silicon carbide coating, a first fixed layer, and a silicon carbide deposition layer deposited during the epitaxial reaction, wherein the thickness of the first fixed layer is 8 μm, and the thickness of the silicon carbide deposition layer is 192 μm;

[0092] S12: removing the first fixed layer and the silicon carbide deposited layer by mechanical grinding and polishing to obtain a graphite ring covered with a silicon carbide coating;

[0093] S13: baking the graphite ring covered with the silicon carbide coating at 1600° C. for 45 min;

[0094] S14: placing the baked graphite ring in the reaction chamber;

[0095] S15: The temperature of the reaction chamber is regulated to 1580°C and the pressure is 100 mbar, and ethylene and trichlorosilane are introduced into the reaction chamber to grow a second fixed layer on the baked graphite ring; wherein the flow rate of ethylene is 120 sccm, the flow rate of trichlorosilane is 300, the C / Si ratio in the fixed layer is 0.8, the temperature of the reaction chamber is 1580°C, the pressure of the reaction chamber is 100 mbar, the growth time of the second fixed layer is 580 s, the thickness of the second fixed layer is 8 μm, and the second cleaning of the graphite ring is completed.

[0096] Example 3

[0097] S11: providing a graphite ring after a silicon carbide epitaxial reaction, wherein the graphite ring participating in the silicon carbide epitaxial reaction has been cleaned twice, and the graphite ring includes a silicon carbide coating, a second fixed layer, and a silicon carbide deposition layer deposited during the epitaxial reaction, wherein the thickness of the second fixed layer is 8 μm, and the thickness of the silicon carbide deposition layer is 192 μm;

[0098] S12: removing the second fixed layer and the silicon carbide deposited layer by mechanical grinding and polishing to obtain a graphite ring covered with a silicon carbide coating;

[0099] S13: baking the graphite ring covered with the silicon carbide coating at 1600° C. for 45 min;

[0100] S14: placing the baked graphite ring in the reaction chamber;

[0101] S15: The temperature of the reaction chamber is regulated to 1580°C and the pressure is 100 mbar, and ethylene and trichlorosilane are introduced into the reaction chamber to grow a third fixed layer on the baked graphite ring; wherein the flow rate of ethylene is 120 sccm, the flow rate of trichlorosilane is 300, the C / Si ratio in the fixed layer is 0.8, the temperature of the reaction chamber is 1580°C, the pressure of the reaction chamber is 100 mbar, the growth time of the third fixed layer is 580 s, the thickness of the third fixed layer is 8 μm, and the third cleaning of the graphite ring is completed.

[0102] Example 4

[0103] S11: providing a graphite ring after a silicon carbide epitaxial reaction, wherein the graphite ring participating in the silicon carbide epitaxial reaction has been cleaned three times, and the graphite ring includes a silicon carbide coating, a third fixed layer, and a silicon carbide deposition layer deposited during the epitaxial reaction, wherein the thickness of the third fixed layer is 8 μm, and the thickness of the silicon carbide deposition layer is 192 μm;

[0104] S12: removing the third fixed layer and the silicon carbide deposited layer by mechanical grinding and polishing to obtain a graphite ring covered with a silicon carbide coating;

[0105] S13: baking the graphite ring with the silicon carbide deposition layer removed at 1600° C. for 45 min;

[0106] S14: placing the baked graphite ring in the reaction chamber;

[0107] S15: The temperature of the reaction chamber is regulated to 1580°C and the pressure is 100 mbar, and ethylene and trichlorosilane are introduced into the reaction chamber to grow a fourth fixed layer on the baked graphite ring; wherein the flow rate of ethylene is 120 sccm, the flow rate of trichlorosilane is 300, the C / Si ratio in the fixed layer is 0.8, the temperature of the reaction chamber is 1580°C, the pressure of the reaction chamber is 100 mbar, the growth time of the fourth fixed layer is 580 s, the thickness of the fourth fixed layer is 8 μm, and the fourth cleaning of the graphite ring is completed.

[0108] Comparative Example 1

[0109] S11: providing a graphite ring after a silicon carbide epitaxial reaction, wherein the graphite ring participating in the silicon carbide epitaxial reaction has been cleaned 4 times, and the graphite ring includes a silicon carbide coating, a fourth fixed layer, and a silicon carbide deposition layer deposited during the epitaxial reaction in sequence, wherein the fourth fixed layer has a thickness of 8 μm, and the silicon carbide deposition layer has a thickness of 192 μm;

[0110] S12: removing the fourth fixed layer and the silicon carbide deposited layer by mechanical grinding and polishing to obtain a graphite ring covered with a silicon carbide coating;

[0111] S13: baking the graphite ring covered with the silicon carbide coating at 1600° C. for 45 min;

[0112] S14: placing the baked graphite ring in the reaction chamber;

[0113] S15: The temperature of the reaction chamber is regulated to 1580°C and the pressure is 100 mbar, and ethylene and trichlorosilane are introduced into the reaction chamber to grow a fifth fixed layer on the baked graphite ring; wherein the flow rate of ethylene is 120 sccm, the flow rate of trichlorosilane is 300, the C / Si ratio in the fixed layer is 0.8, the temperature of the reaction chamber is 1580°C, the pressure of the reaction chamber is 100 mbar, the growth time of the fifth fixed layer is 580 s, the thickness of the fifth fixed layer is 8 μm, and the fifth cleaning of the graphite ring is completed.

[0114] Comparative Example 2

[0115] A graphite ring after a silicon carbide epitaxial reaction is provided, wherein the graphite ring has a silicon carbide coating and a silicon carbide deposition layer deposited during the epitaxial reaction, and the thickness of the silicon carbide deposition layer is 300 μm; the graphite ring is not cleaned, that is, the number of times the graphite ring is cleaned is 0.

[0116] The present application also provides a method for epitaxial growth of silicon carbide, comprising:

[0117] S21: placing the silicon carbide substrate on a graphite ring in a reaction chamber of a hot wall horizontal epitaxial furnace;

[0118] S22: The temperature of the reaction chamber is regulated to 1600°C and the pressure is 100 mbar, and ethylene and trichlorosilane are introduced into the reaction chamber to grow a silicon carbide epitaxial layer on the silicon carbide substrate; wherein the flow rate of ethylene is 120 sccm, the flow rate of trichlorosilane is 300 sccm, the C / Si ratio in the epitaxial layer is 0.8, the growth time of the epitaxial layer is 880 s, and the thickness of the epitaxial layer is 13 μm.

[0119] The graphite rings provided in Examples 1 to 4 and Comparative Examples 1 to 2 were used to grow silicon carbide epitaxial layers according to the above-mentioned silicon carbide epitaxial growth method, and the defect density and doping concentration of the grown silicon carbide epitaxial layers were tested.

[0120] Test Method

[0121] (1) The defect density of the silicon carbide epitaxial layer was tested using a surface defect tester (Candela8520 from KLA-Tencor). The test results of Example 1 are shown in Figure 3 For the test results of comparative example 1, please refer to Figure 4 .

[0122] (2) The mercury probe capacitance voltage method (MCV) was used to test the doping concentration of the silicon carbide epitaxial layer.

[0123] (3) Calculation method of the doping concentration uniformity of the silicon carbide epitaxial layer: standard deviation of the doping concentration of 10 measurement points on the silicon carbide epitaxial layer / arithmetic mean of the doping concentration of 10 measurement points on the silicon carbide epitaxial layer×100%.

[0124] Table 1 shows the parameter settings and test results of Examples 1 to 4 and Comparative Examples 1 to 2.

[0125]

[0126] Result analysis:

[0127] From the test results of Examples 1 to 4 and Comparative Example 1, it can be seen that the graphite ring is cleaned every time the thickness of the deposited layer on the graphite ring reaches 180 to 200 μm. The graphite ring can be used continuously after 1 to 4 cleanings, and the defect density of the epitaxial layer grown is not more than 2.2 cm -2 , the uniformity of doping concentration of epitaxial layer does not exceed 4%; when the graphite ring is cleaned more than 4 times, the defect density of the grown epitaxial layer exceeds 4cm -2 , the uniformity of the doping concentration of the epitaxial layer exceeds 5%, and the service life of the graphite ring reaches the technical limit. If the graphite ring continues to be used, the defects and uniformity of the silicon carbide epitaxial wafer grown will begin to deteriorate.

[0128] It can be seen from the test results of Examples 1 to 4 and Comparative Example 2 that when the thickness of the deposited layer on the graphite ring reaches 300 μm, if the graphite ring is not cleaned, the defects and uniformity of the silicon carbide epitaxial wafer grown by using the graphite ring will begin to deteriorate, and the defect density of the grown epitaxial layer exceeds 3.5 cm -2 , the uniformity of epitaxial layer doping concentration exceeds 4%.

[0129] The above is a detailed introduction to the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for cleaning a carrier, characterized in that: A carrier used for cleaning after epitaxial reaction, wherein the carrier is covered with a coating, and a deposition layer is provided on one side of the coating, and the cleaning method comprises: removing at least a portion of the deposited layer to obtain a carrier covered with a coating; The carrier covered with the coating is subjected to heat treatment and surface treatment to complete the cleaning of the carrier.

2. The method for cleaning a carrier according to claim 1, characterized in that: The surface treatment method comprises: Placing the carrier in the reaction chamber; Allowing a carbon source and a silicon source to flow into the reaction chamber to form a fixed layer on the carrier after the heat treatment; The carbon source includes carbon element, the silicon source includes silicon element, and the ratio of the number of atoms of the carbon element to the number of atoms of the silicon element is in the range of 0.6-1.

3. The method for cleaning a carrier according to claim 2, characterized in that: The deposited layer has a first thickness H1, measured in μm, and the fixed layer has a second thickness H2, measured in μm, satisfying: 18≤H1 / H2≤29.

4. The method for cleaning a carrier according to claim 3, characterized in that: The first thickness H1 is in the range of 180 to 200 μm; and / or, The second thickness H2 is in the range of 7 to 10 μm.

5. The method for cleaning a carrier according to claim 2, characterized in that: The carbon source flow rate ranges from 114 to 150 sccm; and / or, The silicon source flow rate is 300 sccm.

6. The method for cleaning a carrier according to claim 2, characterized in that: The carbon source is selected from at least one of ethylene, acetylene, methane and propane; and / or, The silicon source is selected from at least one of silane or silane derivatives.

7. The method for cleaning a carrier according to claim 2, characterized in that: The temperature of the reaction chamber is 1580-1600° C., and the pressure of the reaction chamber is 90-110 mbar; and / or, The time for forming the fixed layer is 480 to 680 seconds.

8. The method for cleaning a carrier according to claim 1, characterized in that: The heat treatment temperature is 1580-1640°C, and the heat treatment time is 30-60 minutes; and / or, The heat treatment device is selected from an epitaxial furnace; and / or, The heat treatment device is selected from any one of a hot-wall horizontal epitaxial furnace, a warm-wall planetary epitaxial furnace, and a quasi-hot-wall vertical epitaxial furnace.

9. The method for cleaning a carrier according to claim 1, characterized in that: A method for removing at least part of the deposited layer, comprising: The deposited layer is polished to remove at least a portion of the deposited layer.

10. The method for cleaning a carrier according to claim 1, characterized in that: The epitaxial carrier comprises a graphite ring; and / or, The material of the coating is selected from silicon carbide.

11. The method for cleaning a carrier according to claim 1, characterized in that: The number of times of the carrier cleaning treatment is 1 to 4 times.

Citation Information

Patent Citations

  • Cleaning processing method for carrying tray

    CN109427542A

  • Epitaxial furnace cleaning method and device, electronic equipment and storage medium

    CN116791198A

  • Regeneration treatment method of silicon carbide epitaxial old carrying disc

    CN117038539A

  • Preparation method of silicon carbide coating on surface of substrate and tray for epitaxial growth of wafer

    CN117702081A

  • Equipment for removing silicon carbide deposition layer of graphite piece

    CN219359856U