Battery aluminum foil and preparation method thereof
Battery aluminum foil is prepared by hot rolling, ultrasonic vibration cold rolling, recrystallization annealing and corona treatment, and the surface of it is coated with modified coatings, which solves the problem of poor performance of existing battery aluminum foils and achieves high electrochemical performance and The increase in strength extends battery life.
Patent Information
- Application Number
- CN202411040465.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing aluminum foil has poor electrochemical performance, low strength and poor surface quality, which cannot meet the needs of power batteries, affecting battery performance and life.
Battery aluminum foil is prepared by combining hot rolling, ultrasonic vibration cold rolling, recrystallization annealing and corona treatment, and the surface of it is coated with modified coatings to optimize the structure and surface characteristics of the aluminum foil and improve the mechanical and electrochemical properties.
The prepared battery aluminum foil has excellent electrochemical properties, high strength and high surface roughness, which can improve battery performance and extend battery life, and improve the rate performance and corrosion resistance of lithium batteries.
Smart Images

Figure BDA0004972242680000141 
Figure BDA0004972242680000151
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery aluminum foil, and in particular to a battery aluminum foil and a preparation method thereof. Background Art
[0002] Developing new energy vehicles is an important measure to address climate change and promote green development. At present, new energy vehicles are more energy-efficient and pollution-free than traditional gasoline-driven vehicles. In particular, pure electric vehicles driven by power batteries have received unanimous praise from users.
[0003] The power source of electric vehicles is basically lithium-ion power batteries, which are mobile energy sources composed of anodes, cathodes and electrolytes. The positive electrode requires battery aluminum foil, and the quality of the aluminum foil directly affects the performance and life of the battery.
[0004] The existing battery aluminum foil has the disadvantages of poor electrochemical performance, low strength and poor surface quality, and cannot meet the demand of power batteries for battery aluminum foil. Therefore, it is necessary to provide a preparation method of battery aluminum foil and battery aluminum foil to solve the above problems. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a battery aluminum foil, wherein the prepared battery aluminum foil has excellent electrochemical properties, high strength and high surface roughness.
[0006] Another object of the present invention is to provide a battery aluminum foil that can meet the needs of power batteries for battery aluminum foil, improve battery performance, and extend battery life.
[0007] The embodiments of the present invention are implemented by the following technical solutions:
[0008] A method for preparing a battery aluminum foil comprises the following steps:
[0009] S1, hot rolling the aluminum foil blank to obtain an aluminum foil intermediate with a thickness of 3.5-4.1 mm, wherein the hot rolling temperature is 300-330° C.;
[0010] S2, using lubricating oil to perform multiple cold rolling on the aluminum foil intermediate under an ultrasonic vibration system, the vibration frequency is 35-40kHz, and a foil rolled blank with a thickness of 0.35-0.45mm is obtained, wherein when the thickness of the intermediate pass is 0.6-0.9mm, a complete recrystallization annealing is performed under nitrogen protection, and the annealing temperature is 400-450°C;
[0011] S3, foil rolling the foil-rolled blank to obtain an aluminum foil with a thickness of 0.01-0.015 mm, wherein the foil rolling speed is 400-600 m / min;
[0012] S4, performing corona treatment on the aluminum foil, and then coating the modified coating on the surface of the aluminum foil, vacuum drying at a temperature of 75-85° C. for 1-2 hours, and then heating to 130-150° C. for drying for 2-3 hours.
[0013] A battery aluminum foil is made by the above-mentioned battery aluminum foil preparation method.
[0014] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0015] In the present invention, the aluminum foil blank is hot rolled at 300-330°C. The blank is subjected to pressure, and its organizational structure is adjusted, making the organizational structure more uniform, the grains smaller, and the mechanical properties, especially tensile strength and plasticity, are improved; the hardness and toughness of the material are also improved, and it has good wear resistance and corrosion resistance; the surface strength of the material is reduced, the number and time of processing are reduced, and the processing cost is reduced; and the surface glossiness is improved. The use of lubricating oil can prevent aluminum from sticking and prevent surface damage. Cold rolling under ultrasonic vibration conditions can optimize the quality of aluminum foil through micro-control, specifically by improving the reaction between metal and non-metal phases, promoting nano-crystallization, and reducing surface energy, thereby obtaining a smaller particle size and improving the processing performance and mechanical properties of the aluminum foil. Through multiple cold rolling, the aluminum foil is deformed and thinned, and its surface finish is increased, so that the aluminum foil has a uniform thickness and smooth edges. Under nitrogen protection, complete recrystallization annealing at 400-450℃ can eliminate the deformation strengthening effect of aluminum foil, restore the aluminum foil to a relatively soft state, facilitate subsequent processing, improve the formability and processing performance of the aluminum foil, reduce the risk of breakage and rupture, and improve the yield and quality of the product. Foil rolling can further thin the aluminum foil to a predetermined thickness and width.
[0016] By combining corona, modified coating and baking, the surface of aluminum foil can be modified, the surface roughness of aluminum foil can be increased, and the adhesion of pole piece can be enhanced. The modified coating is filled between the active material and the aluminum foil, which can enhance the contact area between the positive active material and the current collector, reduce the interface internal resistance, and improve the consistency of the battery internal resistance. In addition, it can also enhance the internal conduction capacity of current, enhance the rate performance of lithium battery, have good heat dissipation effect, and reduce the influence of high temperature on active material; it can have a certain shielding effect on corrosive medium and improve the anti-corrosion performance. The adhesion of modified coating on the surface of aluminum foil can be improved by vacuum drying at a temperature of 75-85℃ for 1-2h, and then heating to 130-150℃ and drying for 2-3h. DETAILED DESCRIPTION
[0017] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0018] A method for preparing a battery aluminum foil comprises the following steps:
[0019] S1. Hot rolling the aluminum foil blank to obtain an aluminum foil intermediate with a thickness of 3.5-4.1 mm, wherein the hot rolling temperature is 300-330° C. The aluminum foil blank is hot rolled at 300-330° C. The blank is subjected to pressure, and its organizational structure is adjusted, making the organizational structure more uniform and the grains smaller, thereby improving the mechanical properties, especially the tensile strength and plasticity; the hardness and toughness of the material can also be improved, and the material has good wear resistance and corrosion resistance; the surface strength of the material is reduced, the processing quantity and time are reduced, and the processing cost is reduced; and the surface glossiness is improved.
[0020] S2. The aluminum foil intermediate is subjected to multiple cold rollings under an ultrasonic vibration system using lubricating oil, with a vibration frequency of 35-40kHz, to obtain a foil rolled blank with a thickness of 0.35-0.45mm, wherein when the thickness of the intermediate pass is 0.6-0.9mm, a complete recrystallization annealing is performed under nitrogen protection, and the annealing temperature is 400-450°C; the use of lubricating oil can prevent aluminum from sticking and surface damage. Cold rolling under ultrasonic vibration conditions can optimize the quality of aluminum foil through micro-control, specifically by improving the reaction between metal and non-metal phases, promoting nano-crystallization, and reducing surface energy, thereby obtaining a smaller particle size and improving the processing performance and mechanical properties of aluminum foil. Through multiple cold rolling, the aluminum foil is deformed and thinned, while its surface finish is increased, so that the aluminum foil has a uniform thickness and smooth edges. Complete recrystallization annealing at 400-450℃ under nitrogen protection can eliminate the deformation strengthening effect of aluminum foil, restore the aluminum foil to a softer state, facilitate subsequent processing steps, improve the formability and processing performance of the aluminum foil, reduce the risk of breakage and rupture, and improve the yield and quality of the product.
[0021] S3, foil rolling the foil-rolled blank to obtain an aluminum foil with a thickness of 0.01-0.015 mm, wherein the foil rolling speed is 400-600 m / min; foil rolling can further thin the aluminum foil to reach a predetermined thickness and width.
[0022] S4, performing corona treatment on the aluminum foil, and then coating the modified coating on the surface of the aluminum foil, vacuum drying at a temperature of 75-85° C. for 1-2 hours, and then heating to 130-150° C. for drying for 2-3 hours.
[0023] By combining corona, modified coating and baking, the surface of aluminum foil can be modified, the surface roughness of aluminum foil can be increased, and the adhesion of pole piece can be enhanced. The modified coating is filled between the active material and the aluminum foil, which can enhance the contact area between the positive active material and the current collector, reduce the interface internal resistance, and improve the consistency of the battery internal resistance. In addition, it can also enhance the internal conduction capacity of current, enhance the rate performance of lithium battery, have good heat dissipation, reduce the influence of high temperature on active material; it can have a certain shielding effect on corrosive medium and improve the anti-corrosion performance. Drying at different temperatures can enhance the adhesion of modified coating on the surface of aluminum foil.
[0024] Furthermore, the lubricating oil includes base oil and lauric acid, and the mass of the lauric acid is 10-12% of the mass of the base oil. Lauric acid, as an additive, can enhance the lubrication effect of the base oil during the cold rolling process of the aluminum foil intermediate, prevent the aluminum foil intermediate from sticking, and prevent damage to the surface of the aluminum foil intermediate during the cold rolling process.
[0025] Furthermore, in step S4, the corona power is 10 kW and the speed is 100 m / min. Corona can modify the surface of the aluminum foil, enhance the adhesion between the aluminum foil and the active material, and increase the contact area between the aluminum foil and the active material.
[0026] Furthermore, the modified coating comprises, by weight, 5-15 parts of graphene oxide, 5-10 parts of nano carbon black, 20-60 parts of alkylamine, 10-20 parts of maleic anhydride grafted polypropylene and 100-200 parts of sodium carboxymethyl cellulose.
[0027] Graphene has the characteristics of large specific surface area, good conductivity, light weight, etc. It also has a thin thickness and strong adhesion, and has great advantages in improving the performance of lithium-ion batteries. The coating of graphene nanosheets can not only increase the contact area between the electrode material and the aluminum foil, but also enhance its adhesion, which is beneficial to the electrical contact and charge transfer between the two, and can inhibit the corrosion of the aluminum foil during long-term cycles. However, excessive coverage of graphene nanosheets will reduce battery performance due to increased contact between graphene nanosheet layers. The combination of nano-carbon black and graphene to form a co-conductive network effectively makes up for the defect of low interlayer conductivity of graphene nanosheets.
[0028] Since the surface and edge of graphene oxide contain a large number of active oxygen-containing functional groups (hydroxyl, carboxyl and epoxy groups), it has good compatibility with water and certain organic solvents. It also has a high specific surface area and strong van der Waals force, which makes it easy to aggregate into a group in some polymers with weak polarity, affecting its performance. Therefore, alkylamine is selected as a modifier, which can be combined with graphene oxide to increase the interlayer spacing of graphene oxide through the modified intercalation of long-chain alkanes, effectively avoiding the occurrence of stacking, aggregation and agglomeration, thereby improving the compatibility with weak polar matrices. The active oxygen-containing functional groups of graphene oxide act as modified grafting points, react chemically with compound molecules rich in active groups, and form covalent bonds.
[0029] Maleic anhydride grafted polypropylene as an adhesive can enhance the adhesion of graphene oxide and nano carbon black on the surface of aluminum foil. Sodium carboxymethyl cellulose is used as an aqueous solvent to directly blend the raw materials and then apply them on the surface of aluminum foil, which is convenient and simple to operate. In addition, maleic anhydride grafted polypropylene can also be grafted and composited with graphene oxide to improve the barrier properties of the material.
[0030] Among them, the graphene oxide matrix helps to increase the loading and dispersibility of the modified material, thereby improving the performance of the material. Nano-carbon black is embedded in the graphene oxide matrix, which makes the modified material have the function of ion exchange and can be used in water treatment, ion separation and other fields. Due to the conductivity of graphene oxide and the electrochemical activity of nano-carbon black, it can be used as an electrochemical electrode material in supercapacitors, lithium-ion batteries and other fields. The composite of graphene oxide and nano-carbon black can improve catalytic activity and selectivity, and has strong adsorption properties.
[0031] By coating the aluminum foil with modified coating to form a covering layer, not only the contact area between the electrode material and the aluminum foil is increased, but also it can serve as a buffer layer to enhance the adhesion between the two, effectively reduce the resistance, and inhibit the increase of resistance during the charge and discharge process. In addition, it can also prevent the corrosion of the aluminum foil and improve the comprehensive performance of lithium-ion batteries, such as higher rate charge and discharge performance, better safety and longer cycle life.
[0032] Furthermore, the preparation method of the modified coating is as follows: graphene oxide is prepared into a dispersion using an organic solvent, alkylamine is added, stirred, ultrasonicated for 1 hour, reacted at 100-120°C for 20 hours, centrifuged, washed with ethanol until neutral, and dried to obtain material A; sodium carboxymethyl cellulose is prepared into a solution, maleic anhydride grafted polypropylene is added, ultrasonicated for 1-2 hours, and then material A and nano carbon black are added, and ultrasonicated for 2-4 hours.
[0033] When preparing graphene oxide dispersion: graphene oxide and organic solvent are mixed, and ultrasonic treatment is performed at room temperature for 0.5 hours to obtain a uniformly dispersed graphene oxide dispersion. By ultrasonic treatment of the blended graphene oxide aerogel and alkylamine, graphene oxide can be modified to have abundant hydrophobic alkane chains and a special lamellar structure similar to graphene, which can have a certain shielding effect on corrosive media and a certain adhesion to metal substrates, making the coating performance even better.
[0034] Furthermore, the preparation method of graphene oxide is as follows: natural graphene powder is mixed with concentrated sulfuric acid, sodium pernitrate and potassium permanganate are added, reacted at 0°C for 1-3h, heated to 30-35°C for 2-4h, and then heated to 60°C for 1h, hydrogen peroxide is added and allowed to stand for 12h, filtered, washed with distilled water until neutral, and graphene oxide slurry is obtained, which is frozen with liquid nitrogen and placed in a freeze dryer for 2d to obtain graphene oxide aerogel. The liquid nitrogen freezing temperature is -196°C, and the temperature of the freeze dryer is 55°C. This method can increase the number of active functional groups on graphene oxide, increase the active modified grafting points, and improve the modification effect on graphene oxide.
[0035] Furthermore, the organic solvent is N,N-dimethylformamide or N-methylpyrrolidone. The ratio of the organic solvent to the graphene oxide is (10-15) ml: (0.05-0.1) g. In the above organic solvent, the graphene oxide is more evenly dispersed.
[0036] Further, the alkylamine includes one or more of dodecylamine, hexadecylamine and octadecylamine.
[0037] The battery aluminum foil of the present application exhibits significantly enhanced electrochemical performance in terms of internal resistance, specific capacity, rate performance and cycle stability.
[0038] Example 1
[0039] A method for preparing a battery aluminum foil comprises the following steps:
[0040] S1, hot rolling the aluminum foil blank to obtain an aluminum foil intermediate with a thickness of 3.5 mm, wherein the hot rolling temperature is 300° C.;
[0041] S2, using lubricating oil to perform multiple cold rolling on the aluminum foil intermediate under an ultrasonic vibration system, the vibration frequency is 35kHz, and a foil rolled blank with a thickness of 0.35mm is obtained, wherein, when the thickness of the intermediate pass is 0.6mm after cold rolling, a complete recrystallization annealing is performed under nitrogen protection, and the annealing temperature is 400°C;
[0042] S3, foil rolling the foil-rolled blank to obtain an aluminum foil with a thickness of 0.01 mm, wherein the foil rolling speed is 400 m / min;
[0043] S4, corona treatment is performed on the aluminum foil, the corona power is 10 kW, the speed is 100 m / min, and then the modified coating is coated on the surface of the aluminum foil, vacuum dried at a temperature of 75° C. for 1 h, and then heated to 130° C. and dried for 2 h.
[0044] The modified coating includes: 5g of graphene oxide, 5g of nano carbon black, 20g of dodecylamine, 10g of maleic anhydride grafted polypropylene and 100g of sodium carboxymethyl cellulose;
[0045] The preparation method of the modified coating is as follows: graphene oxide and N,N-dimethylformamide are mixed, ultrasonicated at room temperature for 0.5 hours to obtain a uniformly dispersed graphene oxide dispersion, dodecylamine is added, stirred, ultrasonicated for 1 hour, reacted at 100°C for 20 hours, centrifuged, washed with ethanol until neutral, and dried to obtain material A; sodium carboxymethyl cellulose is prepared into a solution, maleic anhydride grafted polypropylene is added, ultrasonicated for 1 hour, and material A and nano carbon black are added, and ultrasonicated for 2 hours;
[0046] The preparation method of graphene oxide is as follows: natural graphene powder is mixed with concentrated sulfuric acid, sodium pernitrate and potassium permanganate are added, reacted at 0°C for 1 hour, heated to 30°C for 2 hours, and further heated to 60°C for 1 hour, hydrogen peroxide is added and allowed to stand for 12 hours, filtered, washed with distilled water until neutral, and graphene oxide slurry is obtained, which is quickly frozen with liquid nitrogen (-196°C) and then placed in a freeze dryer (55°C) for 2 days to obtain graphene oxide aerogel.
[0047] Example 2
[0048] A method for preparing a battery aluminum foil comprises the following steps:
[0049] S1, hot rolling the aluminum foil blank to obtain an aluminum foil intermediate with a thickness of 3.6 mm, wherein the hot rolling temperature is 310° C.;
[0050] S2, using lubricating oil to perform multiple cold rolling on the aluminum foil intermediate under an ultrasonic vibration system, the vibration frequency is 36kHz, and a foil rolled blank with a thickness of 0.38mm is obtained, wherein, when the thickness of the intermediate pass is 0.7mm after cold rolling, a complete recrystallization annealing is performed under nitrogen protection, and the annealing temperature is 410°C;
[0051] S3, foil rolling the foil-rolled blank to obtain an aluminum foil with a thickness of 0.012 mm, wherein the foil rolling speed is 450 m / min;
[0052] S4, corona treatment is performed on the aluminum foil, the corona power is 10 kW, the speed is 100 m / min, and then the modified coating is coated on the surface of the aluminum foil, vacuum dried at a temperature of 78° C. for 1.2 h, and then heated to 135° C. and dried for 2.2 h.
[0053] The modified coating includes: 8g of graphene oxide, 6g of nano carbon black, 25g of dodecylamine, 12g of maleic anhydride grafted polypropylene and 120g of sodium carboxymethyl cellulose;
[0054] The preparation method of the modified coating is as follows: mixing graphene oxide and N-methylpyrrolidone, ultrasonicating at room temperature for 0.5 hours to obtain a uniformly dispersed graphene oxide dispersion, adding dodecylamine, stirring, ultrasonicating for 1 hour, reacting at 105°C for 20 hours, centrifuging, washing with ethanol until neutral, and drying to obtain material A; preparing sodium carboxymethyl cellulose into a solution, adding maleic anhydride grafted polypropylene, ultrasonicating for 1.2 hours, then adding material A and nano carbon black, and ultrasonicating for 2.5 hours;
[0055] The preparation method of graphene oxide is as follows: natural graphene powder is mixed with concentrated sulfuric acid, sodium pernitrate and potassium permanganate are added, the mixture is reacted at 0°C for 1.2 hours, the mixture is heated to 33°C for 2.5 hours, the mixture is further heated to 60°C for 1 hour, hydrogen peroxide is added and allowed to stand for 12 hours, the mixture is filtered, and the mixture is washed with distilled water until it is neutral to obtain graphene oxide slurry, which is then quickly frozen with liquid nitrogen (-196°C) and then placed in a freeze dryer (55°C) for 2 days to obtain graphene oxide aerogel.
[0056] Example 3
[0057] A method for preparing a battery aluminum foil comprises the following steps:
[0058] S1, hot rolling the aluminum foil blank to obtain an aluminum foil intermediate with a thickness of 4 mm, wherein the hot rolling temperature is 320° C.;
[0059] S2, using lubricating oil to perform multiple cold rolling on the aluminum foil intermediate under an ultrasonic vibration system, the vibration frequency is 38kHz, and a foil rolled blank with a thickness of 0.4mm is obtained, wherein when the thickness of the intermediate pass is 0.8mm after cold rolling, a complete recrystallization annealing is performed under nitrogen protection, and the annealing temperature is 440°C;
[0060] S3, foil rolling the foil-rolled blank to obtain an aluminum foil with a thickness of 0.014 mm, wherein the foil rolling speed is 500 m / min;
[0061] S4, corona treatment is performed on the aluminum foil, the corona power is 10 kW, the speed is 100 m / min, and then the modified coating is coated on the surface of the aluminum foil, vacuum dried at a temperature of 80° C. for 1.8 h, and then heated to 145° C. and dried for 2.5 h.
[0062] The modified coating includes: 12g of graphene oxide, 8g of nano carbon black, 50g of hexadecylamine, 15g of maleic anhydride grafted polypropylene and 180g of sodium carboxymethyl cellulose;
[0063] The preparation method of the modified coating is as follows: graphene oxide and N,N-dimethylformamide are mixed, ultrasonicated at room temperature for 0.5 hours to obtain a uniformly dispersed graphene oxide dispersion, hexadecylamine is added, stirred, ultrasonicated for 1 hour, reacted at 115°C for 20 hours, centrifuged, washed with ethanol until neutral, and dried to obtain material A; sodium carboxymethyl cellulose is prepared into a solution, maleic anhydride grafted polypropylene is added, ultrasonicated for 1.8 hours, material A and nano carbon black are added, and ultrasonicated for 3 hours;
[0064] The preparation method of graphene oxide is as follows: natural graphene powder is mixed with concentrated sulfuric acid, sodium pernitrate and potassium permanganate are added, reacted at 0°C for 2h, heated to 33°C for 3h, further heated to 60°C for 1h, hydrogen peroxide is added and allowed to stand for 12h, filtered, washed with distilled water until neutral, to obtain graphene oxide slurry, quickly frozen with liquid nitrogen (-196°C), and then placed in a freeze dryer (55°C) for 2d to obtain graphene oxide aerogel.
[0065] Example 4
[0066] A method for preparing a battery aluminum foil comprises the following steps:
[0067] S1, hot rolling the aluminum foil blank to obtain an aluminum foil intermediate with a thickness of 4.1 mm, wherein the hot rolling temperature is 330° C.;
[0068] S2, using lubricating oil to perform multiple cold rolling on the aluminum foil intermediate under an ultrasonic vibration system, the vibration frequency is 40kHz, and a foil rolled blank with a thickness of 0.45mm is obtained, wherein, when the thickness of the intermediate pass is 0.9mm after cold rolling, a complete recrystallization annealing is performed under nitrogen protection, and the annealing temperature is 450°C;
[0069] S3, foil rolling the foil-rolled blank to obtain an aluminum foil with a thickness of 0.015 mm, wherein the foil rolling speed is 600 m / min;
[0070] S4, corona treatment is performed on the aluminum foil, the corona power is 10 kW, the speed is 100 m / min, and then the modified coating is coated on the surface of the aluminum foil, vacuum dried at a temperature of 85° C. for 2 h, and then heated to 150° C. and dried for 3 h.
[0071] The modified coating includes: 15g of graphene oxide, 10g of nano carbon black, 60g of octadecylamine, 20g of maleic anhydride grafted polypropylene and 200g of sodium carboxymethyl cellulose;
[0072] The preparation method of the modified coating is as follows: graphene oxide and N-methylpyrrolidone are mixed, ultrasonicated at room temperature for 0.5 hours to obtain a uniformly dispersed graphene oxide dispersion, octadecylamine is added, stirred, ultrasonicated for 1 hour, reacted at 120°C for 20 hours, centrifuged, washed with ethanol until neutral, and dried to obtain material A; sodium carboxymethyl cellulose is prepared into a solution, maleic anhydride grafted polypropylene is added, ultrasonicated for 2 hours, and material A and nano carbon black are added, and ultrasonicated for 4 hours;
[0073] The preparation method of graphene oxide is as follows: natural graphene powder is mixed with concentrated sulfuric acid, sodium pernitrate and potassium permanganate are added, reacted at 0°C for 3h, heated to 35°C for 4h, further heated to 60°C for 1h, hydrogen peroxide is added and allowed to stand for 12h, filtered, washed with distilled water until neutral, to obtain graphene oxide slurry, quickly frozen with liquid nitrogen (-196°C), and then placed in a freeze dryer (55°C) for 2d to obtain graphene oxide aerogel.
[0074] Comparative Example 1
[0075] The difference between this comparative example and Example 1 is that no modified coating is applied, and at this time, the surface modification of the aluminum foil is corona + baking.
[0076] Comparative Example 2
[0077] The difference between this comparative example and Example 1 is that no corona treatment is performed.
[0078] Comparative Example 3
[0079] The difference between this comparative example and Example 1 is that the graphene oxide in the modified coating is replaced by natural graphene.
[0080] Comparative Example 4
[0081] The difference between this comparative example and Example 1 is that no nano carbon black is added to the modified coating.
[0082] Comparative Example 5
[0083] The difference between this comparative example and Example 1 is that graphene oxide is not added to the modified coating.
[0084] Comparative Example 6
[0085] The difference between this comparative example and Example 1 is that the graphene oxide is not modified, and the raw materials of the modified coating are directly mixed and then subjected to ultrasonic treatment.
[0086] Comparative Example 7
[0087] The difference between this comparative example and Example 1 is that ultrasonic vibration is not used during the cold rolling process.
[0088] Test results
[0089] The battery aluminum foils prepared in the examples and comparative examples were tested, and the results were as follows:
[0090] Roughness: The surface roughness of the battery aluminum foil was tested using a Japanese Mitutoyo SJ-210 roughness tester.
[0091] Pole piece adhesion: Dongguan Lixian HZ-1007C tensile testing machine was used to test the pole piece adhesion between the pole piece active coating and the aluminum foil. Test method: Make a pole piece specimen with a length of 250mm and a width of 180mm, use 3M tape to stick the pole piece coating, peel it off at 180°, and the stroke is 100m.
[0092] Battery internal resistance: The battery 30% SOC AC internal resistance (ACR) was tested using Changzhou Hepu Electronics HP3554 battery internal resistance tester.
[0093] The corrosion resistance, tensile strength and total elongation at break of aluminum foil were tested in accordance with the GB / T 3198-2010 "Aluminum Foil" standard.
[0094] Table 1 Performance test
[0095]
[0096]
[0097] According to Table 1, the battery aluminum foils prepared in Examples 1-4 have higher surface roughness, greater electrode sheet adhesion, lower battery internal resistance, better tensile strength, total elongation at break and corrosion resistance.
[0098] Compared with Example 1, Comparative Example 1 has poor surface roughness, electrode adhesion, total elongation at break and corrosion resistance. This shows that the modified coating can enhance the surface properties of aluminum foil. Compared with Example 1, Comparative Example 2 has poor surface roughness and electrode adhesion. This shows that corona treatment can enhance the surface roughness and electrode adhesion of aluminum foil. Compared with the examples, Comparative Examples 1-2 can be combined with corona and modified coating to enhance the surface roughness and electrode adhesion of aluminum foil.
[0099] Comparison of Example 3 with Example 1 shows that the electrode adhesion, battery internal resistance and corrosion resistance of Comparative Example 3 are poor. This shows that graphene oxide can enhance the electrode adhesion, reduce the battery internal resistance and enhance the corrosion resistance. The reason may be that graphene oxide has a large number of active functional groups, can be combined with alkylamine and maleic anhydride grafted polypropylene to form a network structure, can load more nano carbon black, and is convenient for forming a stable isolation film on the surface of aluminum foil.
[0100] Compared with Example 1, Comparative Examples 4-5 show that the combination of nano carbon black and graphene oxide can reduce the internal resistance of the battery and improve the corrosion resistance of the aluminum foil. Compared with Example 1, Comparative Example 6 shows that the preparation method of the embodiment can enhance the modification effect of the modified coating on the aluminum foil, making the performance of the aluminum foil more excellent. Compared with Example 1, Comparative Example 7 shows that the mechanical properties of the aluminum foil can be enhanced by ultrasonic vibration-assisted rolling.
[0101] In summary, the present application provides a battery aluminum foil having higher surface roughness, greater electrode sheet adhesion, lower battery internal resistance, better tensile strength, total elongation at break and corrosion resistance.
[0102] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing battery aluminum foil, It is characterized in that The following steps are involved: S1, hot rolling the aluminum foil blank to obtain an aluminum foil intermediate with a thickness of 3.5-4.1 mm, wherein the hot rolling temperature is 300-330° C.; S2, using lubricating oil to perform multiple cold rolling on the aluminum foil intermediate under an ultrasonic vibration system, the vibration frequency is 35-40kHz, and a foil rolled blank with a thickness of 0.35-0.45mm is obtained, wherein when the thickness of the intermediate pass is 0.6-0.9mm, a complete recrystallization annealing is performed under nitrogen protection, and the annealing temperature is 400-450°C; S3, foil rolling the foil-rolled blank to obtain an aluminum foil with a thickness of 0.01-0.015 mm, wherein the foil rolling speed is 400-600 m / min; S4, performing corona treatment on the aluminum foil, then coating the surface of the aluminum foil with a modified coating, vacuum drying at a temperature of 75-85° C. for 1-2 hours, then heating to 130-150° C. for drying for 2-3 hours, to obtain the battery aluminum foil.
2. The method for preparing the battery aluminum foil according to claim 1, It is characterized in that The lubricating oil comprises base oil and lauric acid, and the mass of the lauric acid is 10-12% of the mass of the base oil.
3. The method for preparing the battery aluminum foil according to claim 1, It is characterized in that In step S4, the corona power is 10 kW and the speed is 100 m / min.
4. The method for preparing the battery aluminum foil according to claim 1, It is characterized in that The modified coating comprises, by weight, 5-15 parts of graphene oxide, 5-10 parts of nano carbon black, 20-60 parts of alkylamine, 10-20 parts of maleic anhydride grafted polypropylene and 100-200 parts of sodium carboxymethyl cellulose.
5. The method for preparing the battery aluminum foil according to claim 4, It is characterized in that The preparation method of the modified coating comprises: preparing graphene oxide into a dispersion liquid by using an organic solvent, adding alkylamine, stirring, ultrasonicating for 1 hour, reacting at 100-120° C. for 20 hours, centrifuging, washing with ethanol until neutral, and drying to obtain material A; preparing sodium carboxymethyl cellulose into a solution, adding maleic anhydride grafted polypropylene, ultrasonicating for 1-2 hours, then adding material A and nano carbon black, and ultrasonicating for 2-4 hours.
6. The method for preparing the battery aluminum foil according to claim 4 or 5, It is characterized in that The preparation method of the graphene oxide is as follows: natural graphene powder is mixed with concentrated sulfuric acid, sodium pernitrate and potassium permanganate are added, reacted at 0°C for 1-3h, heated to 30-35°C for 2-4h, further heated to 60°C for 1h, added with hydrogen peroxide and allowed to stand for 12h, filtered, washed with distilled water until neutral, to obtain graphene oxide slurry, quickly frozen with liquid nitrogen, and then placed in a freeze dryer for 2d to obtain graphene oxide aerogel.
7. The method for preparing the battery aluminum foil according to claim 4, It is characterized in that The organic solvent is N,N-dimethylformamide or N-methylpyrrolidone.
8. The method for preparing the battery aluminum foil according to claim 4, It is characterized in that The alkylamine includes one or more of dodecylamine, hexadecylamine and octadecylamine.
9. A battery aluminum foil, It is characterized in that The battery aluminum foil is made according to the preparation method of any one of claims 1 to 8.
Citation Information
Patent Citations
Method for rolling ultra-thin foil by ultrasonic-assisted multi-roller rolling mill
CN108994080A
Carbon-coated aluminum foil for lithium ion batteries
CN109935837A
Preparation method of graphene coating aluminum foil
CN110707328A
Preparation method of soft package battery aluminum foil and soft package battery aluminum foil
CN115198129A
Carbon-coated aluminum foil coating and preparation method and application of carbon-coated aluminum foil
CN116694157A