Preparation method of low-pH-value lithium iron manganese phosphate positive electrode material, electrode and lithium battery

By employing centrifugation and secondary sintering, the high pH and high viscosity issues of lithium manganese iron phosphate cathode materials were addressed, enabling the preparation of low pH and low water absorption lithium manganese iron phosphate cathode materials. This improved processing and electrochemical performance while reducing production costs.

CN118978136APending Publication Date: 2024-11-19HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD

Patent Information

Application Number
CN202411066343.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-16
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The high residual lithium on the surface of lithium manganese iron phosphate cathode material during the preparation process leads to a high pH value, resulting in poor coating effect, easy water absorption, and excessive viscosity in subsequent processes, which affects the processing performance and limits its large-scale application.

Method used

The lithium manganese iron phosphate precursor after primary sintering is ground and centrifuged to separate the precipitated lithium and reduce the pH value of the wet lithium manganese iron phosphate residue after solid-liquid separation. Then, it is sintered again with an appropriate proportion of carbon source to reduce water absorption and viscosity.

Benefits of technology

It effectively reduces the pH value and water absorption of lithium manganese iron phosphate cathode material, lowers the viscosity to 200 mPa·s to 400 mPa·s, improves processing performance, maintains electrochemical performance, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978136A_ABST
    Figure CN118978136A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium batteries, and particularly relates to a preparation method of a low-pH-value lithium iron manganese phosphate positive electrode material, an electrode and a lithium battery, the method comprises the following steps: mixing a lithium source, an iron source, a phosphorus source and a manganese source, and carrying out primary sintering to obtain a lithium iron manganese phosphate precursor; grinding the lithium manganese iron phosphate precursor in a dispersion medium until the particle size of the lithium manganese iron phosphate precursor meets a preset condition to obtain lithium manganese iron phosphate slurry; carrying out centrifugal treatment on the lithium manganese iron phosphate slurry, and carrying out solid-liquid separation to take a solid part, so as to obtain lithium manganese iron phosphate wet slag; the method comprises the following steps: mixing the lithium manganese iron phosphate wet slag, a carbon source and a coating agent in a mixed medium, and sequentially carrying out drying treatment and secondary sintering to obtain the lithium manganese iron phosphate positive electrode material. Compared with the prior art, the method has the advantages that the pH value of the lithium manganese iron phosphate positive electrode material is reduced, the viscosity of the lithium manganese iron phosphate positive electrode material in the subsequent homogenization process is reduced, and the quality of the lithium manganese iron phosphate positive electrode material is improved; and the electrochemical performance at the same level as that in the prior art is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of lithium battery technology, and in particular to a preparation method of a low pH lithium manganese iron phosphate positive electrode material, an electrode, and a lithium battery. Background Art

[0002] At present, the sand grinding process of the lithium iron phosphate precursor of the lithium iron phosphate positive electrode material leads to a high level of residual lithium on the surface of the lithium iron phosphate positive electrode material, which makes the pH value of the lithium iron phosphate positive electrode material high, and then leads to poor coating of the lithium iron phosphate positive electrode material, resulting in easy water absorption. In the subsequent process of homogenization, the viscosity is too high and even gelation occurs, which reduces the processing performance and greatly restricts the large-scale application of the lithium iron phosphate positive electrode material.

[0003] The existing technology has the problem that the pH value of lithium manganese iron phosphate positive electrode material is high and the viscosity is large, resulting in poor processing performance. Summary of the invention

[0004] The embodiments of the present application provide a method for preparing a low-pH lithium iron manganese phosphate positive electrode material, an electrode, and a lithium battery, which can solve the problem that the lithium iron manganese phosphate positive electrode material has a high pH value and high viscosity, resulting in poor processing performance.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising:

[0006] Mixing a lithium source, an iron source, a phosphorus source, and a manganese source, and sintering once to obtain a lithium iron manganese phosphate precursor;

[0007] Grinding the lithium iron manganese phosphate precursor in a dispersion medium until the particle size of the lithium iron manganese phosphate precursor meets a preset condition to obtain a lithium iron manganese phosphate slurry;

[0008] The lithium iron manganese phosphate slurry is centrifuged, and the solid portion is separated from the liquid to obtain the lithium iron manganese phosphate wet slag;

[0009] The lithium iron manganese phosphate wet residue, carbon source and coating agent are mixed in a mixed medium, and dried and sintered twice in sequence to obtain a lithium iron manganese phosphate positive electrode material, wherein the pH value of the lithium iron manganese phosphate positive electrode material is 8.0-9.0.

[0010] The present application provides a preparation method of a lithium iron manganese phosphate positive electrode material. Compared with the prior art, the lithium iron manganese phosphate slurry obtained by grinding a lithium iron manganese phosphate precursor after primary sintering is centrifuged to separate the lithium ferromanganese phosphate positive electrode material from the lithium iron manganese phosphate precipitated during the grinding process, thereby preventing the lithium from remaining on the surface of the lithium iron manganese phosphate positive electrode material. Since the lithium precipitated during the grinding process is separated into the supernatant, the pH value of the solid part (i.e., lithium iron manganese phosphate wet residue) from which lithium is removed after solid-liquid separation is reduced. At the same time, the coating agent can react with the lithium ions on the surface of the lithium iron manganese phosphate wet residue, thereby further reducing the pH value of the lithium iron manganese phosphate wet residue. The lithium iron manganese phosphate wet residue is then mixed with a carbon source in an appropriate proportion and subjected to secondary sintering to reduce the pH value. The pH value of the lithium iron manganese phosphate positive electrode material is reduced from greater than 9 to 8.0-9.0, thereby obtaining a lithium iron manganese phosphate positive electrode material with a low pH value; in addition, due to the appropriate ratio and sintering parameters of the lithium iron manganese phosphate wet slag and the carbon source during the secondary sintering, the coating of carbon on the surface of the lithium iron manganese phosphate is improved, and the water absorption of the lithium iron manganese phosphate positive electrode material is reduced, and the rapid viscosity of the subsequent process is reduced from greater than 9000mPa·s to 200mPa·s-400mPa·s, thereby reducing the viscosity of the lithium iron manganese phosphate positive electrode material in the subsequent slurry process, thereby improving the processing performance of the lithium iron manganese phosphate positive electrode material; and experimental verification shows that the lithium iron manganese phosphate positive electrode material with low pH value and low water absorption prepared in the present application maintains the same level of electrochemical performance as the prior art.

[0011] In a second aspect, an embodiment of the present application provides an electrode comprising a lithium manganese iron phosphate positive electrode material obtained by the preparation method described in any one of the contents of the first aspect.

[0012] The electrode of the present application uses a lithium iron manganese phosphate positive electrode material with a low pH value and low water absorption, which reduces the viscosity of the electrode preparation process, improves the processing performance of the lithium iron manganese phosphate positive electrode material, and reduces the production cost of the electrode.

[0013] In a third aspect, an embodiment of the present application provides a lithium battery, wherein the positive electrode of the lithium battery is made of the lithium iron manganese phosphate positive electrode material described in the second aspect.

[0014] The positive electrode of the lithium battery of the present application is made of a lithium iron manganese phosphate positive electrode material with low pH value and low water absorption. While maintaining the electrochemical properties, the pH value and water absorption of the lithium iron manganese phosphate positive electrode material are reduced, the viscosity of the electrode preparation process is reduced, and the processing performance of the lithium iron manganese phosphate positive electrode material is improved, thereby reducing the production cost of the lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0016] Figure 1 It is a schematic flow chart of a method for preparing a lithium iron manganese phosphate positive electrode material provided in one embodiment of the present application. DETAILED DESCRIPTION

[0017] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0018] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0019] In the present application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can all mean: a, b, c, a~b (i.e. a and b), a~c, b~c, or a~b~c, where a, b, c can be single or multiple, respectively.

[0020] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. For example, without departing from the scope of the implementation regulations of this application, the first XX can also be called the second XX, and similarly, the second XX can also be called the first XX. Therefore, the features defined as "first" and "second" can explicitly or implicitly include one or more of the features.

[0021] The terms used in the embodiments of the present application are only for the purpose of describing specific implementation rules, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the implementation rules of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0022] It should be understood that in the various embodiments of the present application, the size of the serial number of each process does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the implementation regulations of this application.

[0023] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0024] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0025] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0026] Since the specific capacity of lithium iron phosphate cathode materials has basically reached the material limit, the design optimization of battery cells and systems has also gradually approached the limit. Therefore, under the condition of a certain specific capacity, if the energy density of lithium iron phosphate batteries needs to be further improved while maintaining the current safety, it is necessary to start from the direction of improving the voltage platform of the material.

[0027] At present, the sand grinding process of the lithium iron phosphate precursor of the lithium iron phosphate positive electrode material leads to a high level of residual lithium on the surface of the lithium iron phosphate positive electrode material, which makes the pH value of the lithium iron phosphate positive electrode material high, and then leads to poor coating effect of the lithium iron phosphate positive electrode material, causing it to absorb water easily. In the subsequent process of homogenization, the viscosity is too high and even gelation occurs, which reduces the processing performance and greatly restricts the large-scale application of the lithium iron phosphate positive electrode material.

[0028] In order to overcome the above problems, the first aspect of an embodiment of the present application provides a method for preparing a lithium iron manganese phosphate positive electrode material, including: S1, mixing a lithium source, an iron source, a phosphorus source, and a manganese source, and performing a sintering process to obtain a lithium iron manganese phosphate precursor; S2, grinding the lithium iron manganese phosphate precursor in a dispersion medium until the particle size of the lithium iron manganese phosphate precursor meets a preset condition to obtain a lithium iron manganese phosphate slurry; S3, centrifuging the lithium iron manganese phosphate slurry, and performing solid-liquid separation to obtain a solid portion to obtain a lithium iron manganese phosphate wet slag; S4, mixing the lithium iron manganese phosphate wet slag with a carbon source in a mixed medium, and performing a drying process and a secondary sintering process in sequence to obtain a lithium iron manganese phosphate positive electrode material, wherein the pH value of the lithium iron manganese phosphate positive electrode material is 8.0 to 9.0.

[0029] The present application provides a method for preparing a lithium iron manganese phosphate positive electrode material. Compared with the prior art, the lithium iron manganese phosphate slurry is obtained by grinding a lithium iron manganese phosphate precursor after a single sintering until a preset condition is met, wherein the preset condition is that the particle size D50 of the lithium iron manganese phosphate precursor is 0.5 μm to 1.5 μm, and then the lithium iron manganese phosphate slurry is centrifuged to separate the lithium precipitated during the grinding process from the lithium iron manganese phosphate positive electrode material, thereby preventing lithium from remaining on the surface of the lithium iron manganese phosphate positive electrode material, and the content of residual lithium on the surface is reduced from more than 180 ppm to less than 80 ppm; since the lithium precipitated during the grinding process is separated into the supernatant, the pH value of the solid part (i.e., lithium iron manganese phosphate wet residue) from which lithium is removed after solid-liquid separation is reduced, and at the same time, the coating agent can react with the residual lithium ions on the surface of the lithium iron manganese phosphate wet residue, further reducing the pH value of the lithium iron manganese phosphate wet residue, and then the lithium iron manganese phosphate wet residue is mixed with a carbon source in an appropriate proportion, and two The pH value is reduced from greater than 9 to 8.0-9.0 by secondary sintering, thereby obtaining a lithium iron manganese phosphate positive electrode material with a low pH value; in addition, since the lithium iron manganese phosphate wet slag and the carbon source adopt an appropriate ratio and sintering parameters during the secondary sintering, the coating of carbon on the surface of the lithium iron manganese phosphate is improved, and the water absorption of the lithium iron manganese phosphate positive electrode material is reduced, and the rapid viscosity of the subsequent process is reduced from greater than 9000mPa·s to 200mPa·s-400mPa·s, thereby reducing the viscosity of the lithium iron manganese phosphate positive electrode material in the subsequent slurry process, thereby improving the processing performance of the lithium iron manganese phosphate positive electrode material; and experimental verification shows that the lithium iron manganese phosphate positive electrode material with low pH value and low water absorption prepared in the present application maintains the electrochemical performance at the same level as the prior art, wherein the 0.1C charging gram capacity reaches 157.5mAh / g, the 0.1C discharging gram capacity reaches 152.11mAh / g, and the 1C discharging gram capacity reaches 143.54mAh / g.

[0030] In some embodiments, the supernatant after centrifugation for solid-liquid separation can be recycled. When the lithium content reaches a certain concentration, a lithium extraction process can be carried out to achieve the recycling of water and lithium elements, further reducing the production cost of the preparation method of the lithium iron manganese phosphate cathode material. Among them, the parameters of the centrifugation treatment are as follows: the centrifugation speed is 1000 rpm to 2500 rpm, and the centrifugation duration is 0.5 h to 2 h. Using the centrifugation treatment parameters of this embodiment can separate the lithium iron manganese phosphate wet slag and the liquid in the lithium iron manganese phosphate slurry as much as possible, so as to separate the lithium precipitated during the grinding process into the supernatant, reducing the pH value of the lithium iron manganese phosphate wet slag after solid-liquid separation. Further, the centrifugation speed is 1500 rpm to 2000 rpm, and the centrifugation duration is 1.0 h to 1.5 h, which can balance the production efficiency and the separation situation, and further separate the lithium precipitated during the grinding process into the supernatant, thereby reducing the pH value of the lithium iron manganese phosphate wet slag after solid-liquid separation.

[0031] In some embodiments, the molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source, and phosphorus in the phosphorus source is (1.0 to 1.05):0.6:0.4:1.03. Mixing lithium, manganese, iron, and phosphorus in the raw materials according to the molar ratio in this embodiment can balance the advantages of lithium iron phosphate and lithium manganese phosphate, thereby improving the electrochemical performance of lithium iron manganese phosphate.

[0032] In some embodiments, the structural general formula of the lithium iron manganese phosphate precursor and the lithium iron manganese phosphate cathode material is LiMn x Fe (1-x) PO4, where 0.5 < X < 0.9. Since the ratio of manganese (Mn) and iron (Fe) in lithium iron manganese phosphate will affect the performance of the lithium iron manganese phosphate cathode material, the ratio of manganese (Mn) and iron (Fe) needs to be set according to the battery requirements to improve the performance of the lithium battery as much as possible.

[0033] In some embodiments, the manganese source is one or a combination of manganese tetroxide, manganese dioxide, manganese oxide, and manganese carbonate; and / or, the iron source is one or a combination of ferric oxide, ferroferric oxide, iron phosphate, iron monoxide, ferrous oxalate, and ferrous acetate; and / or, the phosphorus source is one or a combination of lithium dihydrogen phosphate, sodium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, potassium phosphate, and phosphoric acid; and / or, the lithium source is one or a combination of lithium carbonate, lithium hydroxide, and lithium dihydrogen phosphate.

[0034] In this embodiment, a certain amount of manganese element is added to the lithium iron phosphate positive electrode material, and the synthesized lithium iron manganese phosphate has a higher voltage platform, which can reach about 4.1V, while lithium iron phosphate is about 3.4V to 3.5V. The two positive electrode materials have the same theoretical gram capacity. Due to the higher voltage, the theoretical energy density of lithium iron manganese phosphate is 15% to 20% higher than that of lithium iron phosphate under the same conditions; multiple sources of iron sources can select one or more combinations according to needs to prepare lithium iron manganese phosphate positive electrode materials; multiple sources of phosphorus sources can select one or more combinations according to needs to prepare lithium iron manganese phosphate positive electrode materials; multiple sources of lithium sources can select one or more combinations according to needs to prepare lithium iron manganese phosphate positive electrode materials; multiple sources of the above raw materials can also reduce production costs.

[0035] In some embodiments, the parameters of the primary sintering are: sintering temperature is 400℃~700℃, heating rate is 3℃~10℃, and sintering time is 4h~9h; the heating rate of this embodiment allows the mixture of lithium source, iron source, phosphorus source, and manganese source to be evenly heated for reaction; the sintering temperature of this embodiment allows the mixture of lithium source, iron source, phosphorus source, and manganese source to react at a suitable reaction speed, and a sintering temperature that is too low will result in a slow reaction speed, a long sintering time, or a sintering temperature that is too high will result in a too fast reaction speed, which will cause incomplete reaction and too many impurities; the sintering time is convenient for the mixture of lithium source, iron source, phosphorus source, and manganese source to react completely as much as possible under the heating rate and sintering temperature of this embodiment, so as to improve the performance of the lithium iron manganese phosphate positive electrode material. Further, the parameters of the primary sintering are: sintering temperature is 500℃~600℃, heating rate is 5℃, and sintering time is 6h~7h, which is more conducive to reduction reaction and primary carbon coating.

[0036] In some embodiments, the solid content of the lithium manganese iron phosphate precursor during grinding is 10% to 60%, and the dispersion medium for grinding is water; grinding the lithium manganese iron phosphate precursor in water with the solid content of this embodiment can make the lithium manganese iron phosphate precursor more evenly stressed during grinding, and the particle size after grinding is more uniform, which is convenient for subsequent process treatment.

[0037] In some embodiments, the carbon source is one or more combinations of glucose, sucrose, lactose, maltose, phenolic resin, carbon nanotubes and epoxy resin; the carbon source of this embodiment is diversified and can be selected according to needs. The carbon source is used to coat the lithium iron manganese phosphate particles in the secondary sintering, increase the conductivity of the lithium iron manganese phosphate positive electrode material, and reduce the water absorption of the lithium iron manganese phosphate positive electrode material, thereby reducing the viscosity of the subsequent lithium iron manganese phosphate positive electrode material processing technology, thereby reducing the production cost of the lithium battery.

[0038] In some embodiments, the carbon content of the lithium iron manganese phosphate positive electrode material is 1.4% to 1.7%, or the mass ratio of lithium iron manganese phosphate wet slag to the carbon source is 20: (1 to 4). The carbon content of this embodiment allows the carbon to increase the conductivity of the lithium iron manganese phosphate when the carbon is coated with the lithium iron manganese phosphate, without reducing the conductivity of lithium ions and manganese ions; too little carbon content will reduce the conductivity of carbon, and too much carbon content will reduce the conductivity of lithium ions and manganese ions.

[0039] In some embodiments, the mixed medium is water, and the parameters of the secondary sintering are: sintering temperature of 600°C to 1000°C, heating rate of 3°C to 10°C, and sintering time of 5h to 10h; the heating rate of this embodiment can allow the mixture of lithium source, iron source, phosphorus source, and manganese source to be uniformly heated and reacted at a slower rate than the primary sintering; the sintering temperature of this embodiment can allow the mixture of lithium iron manganese phosphate wet slag and carbon source to react at an appropriate reaction rate. If the sintering temperature is too low, the reaction rate will be too slow and the sintering time will be too long, or if the sintering temperature is too high, the reaction rate will be too fast, resulting in incomplete reaction and too many impurities; the sintering time is convenient for the mixture of lithium iron manganese phosphate wet slag and carbon source to react as completely as possible under the conditions of the heating rate and sintering temperature of this embodiment, thereby improving the coating of the carbon source and improving the performance of the lithium iron manganese phosphate positive electrode material. Furthermore, the parameters of the secondary sintering are: sintering temperature of 700°C to 800°C, heating rate of 5°C, and sintering time of 6h to 8h, which improve the coating integrity of the secondary carbon coating.

[0040] In order to make the above implementation details and operations of the present application clearly understood by those skilled in the art, as well as to demonstrate the significant improvement in the performance of the preparation method of the lithium manganese iron phosphate positive electrode material, the electrode and the lithium battery in the embodiment of the present application, the above technical scheme is illustrated by multiple embodiments below.

[0041] Example 1

[0042] A preparation method of a lithium iron manganese phosphate positive electrode material comprises: weighing lithium carbonate, manganese trioxide, ferric oxide and phosphoric acid according to a molar ratio of Li:Mn:Fe:P of 1.03:0.6:0.4:1 and mixing them; then performing a primary sintering to obtain a lithium iron manganese phosphate precursor, wherein the primary sintering temperature is 600°C; adding water to the lithium iron manganese phosphate precursor according to a solid content of 50% and grinding it to a certain particle size, using a centrifuge to perform solid-liquid separation, mixing the obtained lithium iron manganese phosphate wet residue with glucose and water, drying it, and performing a secondary sintering, wherein the secondary sintering temperature is 750°C, to obtain a carbon-coated lithium iron manganese phosphate positive electrode material.

[0043] Example 2, compared with Example 1, mainly the molar ratio of lithium manganese iron phosphorus is different

[0044] A method for preparing a lithium iron manganese phosphate positive electrode material comprises: weighing lithium carbonate, manganese trioxide, ferric oxide and phosphoric acid according to a molar ratio of Li:Mn:Fe:P of 1.02:0.6:0.4:1 and mixing them; then performing a primary sintering to obtain a lithium iron manganese phosphate precursor, wherein the primary sintering temperature is 600°C; adding water to the precursor according to a solid content of 50%, grinding the precursor to the same particle size as in Example 1, performing solid-liquid separation by using a centrifuge, mixing the obtained lithium iron manganese phosphate wet residue with glucose and water, drying, and performing a secondary sintering, wherein the secondary sintering temperature is 750°C, to obtain a carbon-coated lithium iron manganese phosphate positive electrode material.

[0045] Comparative Example 1

[0046] A method for preparing a lithium iron manganese phosphate positive electrode material comprises: weighing lithium carbonate, manganese trioxide, ferric oxide and phosphoric acid according to a molar ratio of Li:Mn:Fe:P of 1.03:0.6:0.4:1 for mixing; then performing a primary sintering to obtain a lithium iron manganese phosphate precursor, wherein the primary sintering temperature is 600°C; mixing the precursor with glucose and water to grind to the same particle size as in Example 1; drying; and then performing a secondary sintering, wherein the secondary sintering temperature is 750°C, to obtain a carbon-coated lithium iron manganese phosphate positive electrode material.

[0047] Comparative Example 2

[0048] A method for preparing a lithium iron manganese phosphate positive electrode material comprises: weighing lithium carbonate, manganese trioxide, ferric oxide, and phosphoric acid according to a molar ratio of Li:Mn:Fe:P of 1.02:0.6:0.4:1, mixing the mixture, and then sintering the mixture once to obtain a lithium iron manganese phosphate precursor at a sintering temperature of 600°C; mixing the precursor with glucose and water to obtain a particle size the same as that in Example 1; drying the mixture, and then sintering the mixture twice at a sintering temperature of 750°C to obtain a carbon-coated lithium iron manganese phosphate positive electrode material.

[0049] Comparative Example 3

[0050] A method for preparing a lithium iron manganese phosphate positive electrode material comprises: weighing lithium carbonate, manganese trioxide, ferric oxide, and phosphoric acid according to a molar ratio of Li:Mn:Fe:P of 1.02:0.6:0.4:1, mixing the mixture, and then sintering the mixture once to obtain a lithium iron manganese phosphate precursor at a sintering temperature of 600°C, mixing the precursor with glucose and water to grind the mixture to the same particle size as in Example 1, drying the mixture, and then sintering the mixture twice at a sintering temperature of 780°C to obtain a carbon-coated lithium iron manganese phosphate positive electrode material.

[0051] Data testing:

[0052] The lithium manganese iron phosphate positive electrode materials prepared in Examples 1 and 2 and Comparative Examples 1, 2 and 3 were subjected to pH value test, surface residual lithium content test, rapid viscosity test, 0.1C charge gram capacity test, 0.1C discharge gram capacity test and 1C discharge gram capacity test. The comparative test data are detailed in Table 1.

[0053] Table 1 Performance test data of lithium manganese iron phosphate positive electrode materials in various embodiments and comparative examples

[0054]

[0055] It can be seen from Table 1 that compared with the traditional two-stage process of Comparative Examples 1, 2, and 3, after centrifugal solid-liquid separation, the pH value, surface residual lithium content, and rapid viscosity of the lithium iron manganese phosphate positive electrode material obtained in Examples 1 and 2 are significantly reduced, and the electrochemical performance of 0.1C charge gram capacity, 0.1C discharge gram capacity, and 1C discharge gram capacity does not decrease, thereby solving the problem of poor processing performance caused by the high pH value and high viscosity of the lithium iron manganese phosphate positive electrode material.

[0056] It should be understood that the size of the serial numbers of the steps in the above embodiments does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0057] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0058] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing a lithium manganese iron phosphate positive electrode material, It is characterized in that include: S1, mixing a lithium source, an iron source, a phosphorus source, and a manganese source, and sintering them once to obtain a lithium iron manganese phosphate precursor; S2, grinding the lithium iron manganese phosphate precursor in a dispersion medium until the particle size of the lithium iron manganese phosphate precursor meets a preset condition to obtain a lithium iron manganese phosphate slurry; S3, centrifuging the lithium iron manganese phosphate slurry, and performing solid-liquid separation to obtain a solid portion to obtain lithium iron manganese phosphate wet slag; S4, mixing the lithium iron manganese phosphate wet residue, the carbon source and the coating agent in a mixed medium, and sequentially performing drying treatment and secondary sintering to obtain a lithium iron manganese phosphate positive electrode material, wherein the pH value of the lithium iron manganese phosphate positive electrode material is 8.0-9.

0.

2. The preparation method according to claim 1, It is characterized in that The molar ratio of lithium in the lithium source, manganese in the manganese source, iron in the iron source, and phosphorus in the phosphorus source is (1.0-1.05):0.6:0.4:1.

03.

3. The preparation method according to claim 1, It is characterized in that The manganese source is one or more combinations of manganese tetraoxide, manganese dioxide, manganese oxide, and manganese carbonate; And / or, the iron source is one or more combinations of ferrous oxide, ferrous oxide, ferric phosphate, ferric oxide, ferrous oxalate and ferrous acetate; And / or, the phosphorus source is one or more combinations of lithium dihydrogen phosphate, sodium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, potassium phosphate, and phosphoric acid; And / or, the lithium source is one or more combinations of lithium carbonate, lithium hydroxide, and lithium dihydrogen phosphate.

4. The preparation method according to claim 1, It is characterized in that The parameters of the primary sintering are as follows: the sintering temperature is 400° C. to 700° C., and the sintering time is 4 h to 9 h; The preset condition is that the particle size D50 of the lithium manganese iron phosphate precursor is 0.5 μm to 1.5 μm.

5. The preparation method according to claim 1, It is characterized in that The solid content of the lithium manganese iron phosphate precursor during grinding is 10% to 60%, and the dispersion medium during grinding is water.

6. The preparation method according to claim 1, It is characterized in that The carbon source is one or more combinations of glucose, sucrose, lactose, maltose, phenolic resin, carbon nanotubes and epoxy resin; The carbon content of the lithium manganese iron phosphate positive electrode material is 1.4% to 1.7%.

7. The preparation method according to claim 1, It is characterized in that The mixed medium is water, and the parameters of the secondary sintering are: sintering temperature is 600° C. to 1000° C., and sintering time is 5 h to 10 h; The coating agent is at least one of iron phosphate, aluminum phosphate, manganese carbonate, cobalt oxide, and titanium dioxide, and is used to react with residual lithium ions on the surface of the lithium manganese iron phosphate wet slag to generate active components corresponding to the coating agent.

8. The preparation method according to claim 1, It is characterized in that The general structural formula of the lithium iron manganese phosphate precursor and the lithium iron manganese phosphate positive electrode material is LiMn x Fe (1-x) PO4, of which 0.5 <X<0.9。 9. An electrode, It is characterized in that The invention comprises a lithium manganese iron phosphate positive electrode material obtained by the preparation method according to any one of claims 1 to 8.

10. A lithium battery, It is characterized in that The positive electrode of the lithium battery is made of the lithium iron manganese phosphate positive electrode material as claimed in claim 9.

Citation Information

Patent Citations

  • Lithium manganese iron phosphate positive electrode material and application thereof

    CN116534828A

  • Ternary co-doped modified nano lithium manganese iron phosphate positive electrode material and preparation method thereof

    CN117682496A

  • Lithium iron manganese phosphate positive electrode material and preparation method therefor and use thereof

    WO2024082539A1

Cited By

  • Preparation method of high-compaction lithium manganese iron phosphate positive electrode material

    CN119786544A