Preparation method of supported rare earth hexaboride nano material

By mechanochemically grinding rare earth and boron precursors in a ball mill, combined with alkaline liquid treatment, the harsh reaction conditions and waste resources in the traditional preparation of rare earth hexaborides are solved, and the high efficiency and low efficiency of rare earth hexaboride nanomaterials are achieved. Cost-preparation and high activity, suitable for photothermal catalysts.

CN118978167APending Publication Date: 2024-11-19SHAOXING INST OF NEW ENERGY & MOLECULAR ENG SHANGHAI JIAO TONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411061424.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The traditional method of preparing rare earth hexaboride (LnB6) has problems such as harsh reaction conditions, high equipment costs, complex processes and waste of resources, making it difficult to achieve simple and efficient preparation.

Method used

Using mechanochemical method, the loaded rare earth hexaboride nanomaterial was prepared by using zirconia balls as grinding medium in a planetary mill, and the rare earth precursor, boron precursor and aluminum powder were used, combined with alkaline liquid washing and drying.

Benefits of technology

Large-scale synthetic loaded rare earth hexaboride nanomaterials under mild conditions have small particle size, high activity, simple process, great industrial application value, and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978167A_ABST
    Figure CN118978167A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a supported rare earth hexaboride nano material, and relates to the technical field of material preparation, and the preparation method comprises the following steps: (1) weighing a rare earth precursor, a boron precursor and a reducing agent in sequence according to a certain stoichiometric ratio, taking a zirconium oxide ball as a grinding medium, and then placing in a grinding tank; (2) the grinding tank filled with the sample is placed in a planetary ball mill for ball milling, the rotating speed of the ball mill is 400-600 r / min, and the ball milling time is set to be 15-60 h; and (3) washing the ball-milled product with alkali liquor and deionized water in sequence, and then drying to obtain the supported rare earth hexaboride nanometer material which is small in particle size and high in activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material preparation, and in particular to a method for preparing a supported rare earth hexaboride nanomaterial. Background Art

[0002] Rare earth hexaboride (LnB6) is an important cathode material for thermionic emission sources. LnB6 belongs to the cubic CsCl crystal structure. The rare earth atoms Ln occupy the vertices of the cubic lattice, and six smaller B atoms form an octahedral network structure in the cubic lattice. This unique grid structure, combined with the special 4f orbital of rare earth elements and the electron-deficient characteristics of boron, makes LnB6 have many excellent physical and chemical properties, such as low work function, high conductivity, high carrier concentration, metallic properties, chemical stability, and resistance to thermal radiation. In recent years, studies have found that LnB6 has a strong localized surface plasmon resonance effect near 1000nm near-infrared, and compared with Au nanorods, LnB6 exhibits better photothermal conversion performance. This unique property makes LnB6 expected to become an efficient photothermal catalyst and be applied to various chemical reactions. However, the traditional method of synthesizing LnB6 has problems such as harsh reaction conditions, high equipment costs, and complex processes. Therefore, how to prepare LnB6 simply and efficiently is a major challenge currently faced.

[0003] At present, the synthesis methods for preparing LnB6 include solid phase method, liquid phase method and gas phase method. In the solid phase preparation process, lanthanum chloride and oxide are mainly used as lanthanum sources, B2O3, H3BO3, elemental B and NaBH4 are used as boron sources to prepare LaB6 through high temperature reaction. Later, someone reported the preparation of LaB6 by carbon thermal reduction, which requires 1350-1400℃ to achieve. The gas phase preparation of LaB6 is mainly chemical vapor deposition (CVD), using LaCl3 or La as lanthanum source, BCl3 as boron source, and high temperature reaction in H2 / N2 / Ar atmosphere, and the prepared LaB6 is mainly nanowires and nanotubes. However, due to the high toxicity of BCl3 and the high reaction temperature (>1000℃), the gas phase method has not been widely used in the preparation of LnB6. Compared with the solid phase method and the gas phase method, the liquid phase method mainly uses molten salt to achieve the preparation of LaB6 at low temperature, that is, the lanthanum source and the boron source are mixed with molten salt, and LaB6 nanoparticles can be obtained under conditions below 1000°C. This method is simple in process and has a small LaB6 particle size, but it requires a large amount of molten salt, which is seriously wasteful and requires post-processing. Based on a series of problems in the above-mentioned preparation methods, the development of new preparation technologies is the key to solving these process problems. Summary of the invention

[0004] In view of a series of problems existing in the existing preparation process, the present invention provides a method for preparing supported rare earth hexaboride nanomaterials by a mechanochemical method, which is of great significance for the later development of highly active LnB6 photothermal catalysts.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A method for preparing a supported rare earth hexaboride nanomaterial comprises the following steps:

[0007] (1) weighing a rare earth precursor, a boron precursor and a reducing agent in sequence according to a certain stoichiometric ratio, using zirconium oxide balls as grinding media, and then placing them in a grinding jar;

[0008] (2) placing the sample-filled grinding jar in a planetary ball mill for ball milling at a speed of 400-600 r / min and a ball milling time of 15-60 h;

[0009] (3) The ball-milled product is washed with alkaline solution and deionized water in sequence, and then dried to obtain a supported rare earth hexaboride nanomaterial.

[0010] Further settings are as follows:

[0011] In step (1):

[0012] The rare earth element types contained in the rare earth precursor include but are not limited to one of La, Ce, Pr, Nd, Sm or Eu.

[0013] The rare earth precursor includes, but is not limited to, one or more of rare earth oxides, rare earth hydroxides, rare earth carbonates, and rare earth oxalates.

[0014] The boron precursor includes, but is not limited to, one or more of boron trioxide, elemental boron powder, sodium borohydride / potassium borohydride, and sodium metaborate.

[0015] The reducing agent is Al powder.

[0016] The molar ratio of the rare earth atoms, boron atoms and aluminum atoms is 1:6:7-15.

[0017] The grinding medium is a zirconia ball with a diameter of 5-10 mm.

[0018] The ball-to-material mass ratio is most preferably 5-10:1.

[0019] In step (2):

[0020] The ball milling is carried out under a protective atmosphere, which is argon.

[0021] The rotation speed of the ball mill is 400-600 r / min, preferably 600 r / min; the ball milling time is 15-60 h, preferably 30 h.

[0022] In step (3):

[0023] The alkali solution is preferably an aqueous solution of sodium hydroxide, with a concentration of 1-3 mol / L, preferably 3 mol / L. The drying temperature is 70° C., and the drying time is 8 hours.

[0024] The present invention uses rare earth precursors and boron precursors as raw materials, Al powder as a reducing agent, and adopts a mechanochemical method to prepare LnB6 nanomaterials. The mechanochemical method is one of the important ways to prepare new high-activity materials. Under the action of high-energy ball milling, the particle size of the powder is significantly reduced, the specific surface area of ​​the powder is significantly increased, and the reaction process between substances is greatly accelerated.

[0025] The second aspect of the present invention is to provide an application of the above-prepared supported rare earth hexaboride nanomaterial in a catalyst carrier for photothermal ammonia synthesis reaction.

[0026] The method of the present invention has the following beneficial effects: the present invention realizes large-scale synthesis of supported rare earth hexaboride nanomaterials under mild conditions, reducing energy consumption. The synthesized supported rare earth hexaboride nanomaterial has a small particle size and high activity. The present invention has a simple process, is easy to operate, and has great industrial application value.

[0027] The following is a further description of the implementation scheme of the present invention in conjunction with the accompanying drawings. The following examples are implemented on the premise of the scheme of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the above-mentioned examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the XRD spectrum of the supported LaB6 nanomaterial prepared in Example 1.

[0029] Figure 2 This is the TEM image of the supported LaB6 nanomaterial prepared in Example 1. DETAILED DESCRIPTION

[0030] Example 1

[0031] (1) La2O3, B2O3 and Al were weighed according to the molar ratio of rare earth atoms, boron atoms and aluminum atoms of 1:6:12, loaded in a glove box, and then placed in a 250 mL grinding jar. Zirconia balls were used as grinding media. The diameters of the zirconia balls were 5, 8, and 10 mm, and their mass ratio was 5:3:2. The mass ratio of the zirconia balls to the reaction materials was controlled to be 10:1.

[0032] (2) The ball mill jar containing the sample was placed in a planetary ball mill for ball milling in an Ar atmosphere. The speed of the ball mill was 600 r / min, the ball milling time was set to 30 h, and sampling was performed.

[0033] (3) The ball-milled product was washed with a 3 mol / L sodium hydroxide aqueous solution, centrifuged, and then washed with deionized water for a cycle until the washing solution became neutral. After the last centrifugation, the sample was placed in an oven for drying at 70°C for 8 h to obtain a supported rare earth hexaboride nanomaterial Al2O3-LaB6.

[0034] Product Confirmation:

[0035] like Figure 1-Figure 2 As shown, the supported Al2O3-LaB6 nanomaterial was successfully prepared using the method involved in this patent. In Example 1, Al2O3-supported LaB6 was obtained, and the particle size was about 80nm.

[0036] Alternative Embodiments

[0037] The preparation method described in Example 1 was adopted, and the process parameters of steps 1-3 were adjusted respectively, and their effects on the particle size of the product were tested, as shown in Table 1.

[0038] Embodiment 2-4

[0039] The preparation method is the same as that in Example 1, except that: in step (1), the molar ratios of rare earth lanthanum atoms, boron atoms and aluminum atoms in the raw materials are adjusted to 1:6:7, 1:6:10 and 1:6:15 respectively. La2O3, B2O3 and Al are weighed.

[0040] Embodiment 5-6

[0041] The preparation method is the same as that of Example 1, except that in step (1), the ball-to-material ratio is adjusted to 20:1 and 5:1 respectively.

[0042] Embodiment 7-8

[0043] The preparation method is the same as that in Example 1, except that in step (2), the rotation speed of the ball mill is adjusted to 400 r / min and 500 r / min respectively.

[0044] Table 1. Effects of different process conditions on the particle size of nanomaterials

[0045] Serial number Process conditions Product particle size Example 2 La:B:Al=1:6:7 120nm Example 3 La:B:Al=1:6:10 112nm Example 4 La:B:Al=1:6:15 60nm Example 5 Ball to material ratio 20:1 68nm Example 6 Ball to material ratio 5:1 150nm Example 7 Ball mill speed 400r / min 140nm Example 8 Ball mill speed 500r / min 128nm .

[0046] As shown in Table 1:

[0047] In the preparation method involved in this patent, the loading amount and particle size of the obtained supported hexaboride on the alumina carrier can be adjusted by adjusting the preparation process. Specifically, according to the comparison between Example 1 and Examples 2-4, it can be seen that the Al content has a significant effect on the particle size of the supported hexaboride. According to the comparison between Example 1 and Examples 5-6, it can be seen that increasing the mass ratio of zirconium oxide balls to reactant materials can reduce the particle size of LnB6; according to the comparison between Example 1 and Examples 7-8, it can be seen that increasing the rotation speed of the ball mill can make the prepared particle size smaller.

[0048] Example 9

[0049] The preparation method is the same as that in Example 1, except that: in step (a), the raw materials are adjusted to La2O3, B and Al, and the molar ratio of rare earth atoms, boron atoms and aluminum atoms is the same as that in Example 1.

[0050] Example 10

[0051] The preparation method is the same as that in Example 1, except that in step (a), the raw materials are adjusted to LaCl3, NaBH4 and Al, and the molar ratio of rare earth atoms, boron atoms and aluminum atoms is the same as that in Example 1.

[0052] Embodiment 11

[0053] The preparation method is the same as that in Example 1, except that in step (a), the raw materials are adjusted to La(OH)3, NaBO2 and Al, and the molar ratio of rare earth atoms, boron atoms and aluminum atoms is the same as that in Example 1.

[0054] Example 12

[0055] The preparation method is the same as that in Example 1, except that: in step (a), the raw materials are adjusted to La2(C2O4)3, NaBO2 and Al, and the molar ratio of rare earth atoms, boron atoms and aluminum atoms is the same as that in Example 1.

[0056] Embodiment 13

[0057] The preparation method is the same as that in Example 1, except that: in step (a), the raw materials are adjusted to La2(CO3)3, NaBO2 and Al, and the molar ratio of rare earth atoms, boron atoms and aluminum atoms is the same as that in Example 1.

[0058] Embodiment 14

[0059] The preparation method is the same as that of Example 1, except that in step (1), the type of rare earth element is changed to CeO2 to prepare a supported Al2O3-CeB6 nanomaterial.

[0060] Embodiment 15

[0061] The preparation method is the same as that of Example 1, except that in step (1), the type of rare earth element is changed to Pr2O3 to prepare a supported Al2O3-PrB6 nanomaterial.

[0062] Example 16

[0063] The preparation method is the same as that of Example 1, except that in step (1), the type of rare earth element is changed to Nd2O3 to prepare a supported Al2O3-NdB6 nanomaterial.

[0064] Embodiment 17

[0065] The preparation method is the same as that in Example 1, except that in step (1), the type of rare earth element is changed to Sm2O3 to prepare a supported Al2O3-SmB6 nanomaterial.

[0066] Embodiment 18

[0067] The preparation method is the same as that of Example 1, except that in step (1), the type of rare earth element is changed to Eu2O3 to prepare a supported Al2O3-EuB6 nanomaterial.

[0068] It can be seen from Examples 9-13 that:

[0069] By changing the reactant raw materials, the supported Al2O3-LaB6 nanomaterial shown in Example 1 can still be prepared in one step using the mechanochemical method, which greatly highlights the great potential of the mechanochemical method in the preparation of this type of hexaboride.

[0070] It can be seen from Examples 14-18 that:

[0071] The mechanochemical method proposed in this patent can also be used to successfully prepare a variety of supported rare earth hexaborides, including but not limited to supported Al2O3-LaB6 nanomaterials, supported Al2O3-CeB6 nanomaterials, supported Al2O3-PrB6 nanomaterials, supported Al2O3-NdB6 nanomaterials, supported Al2O3-SmB6 nanomaterials, and supported Al2O3-EuB6 nanomaterials, indicating that the preparation method has a certain universality and can be extended to other hexaboride systems.

[0072] Application Example 1:

[0073] The supported LnB6-Al2O3 nanomaterial prepared in Example 1 was used as a catalyst support for the photothermal ammonia synthesis reaction, and its photothermal ammonia synthesis activity was tested.

[0074] The experimental method is as follows:

[0075] Take 90mg LnB6-Al2O3 and 21mg Ru3(CO) 12After grinding, the temperature was raised to 250°C at a heating rate of 0.5°C / min in a tubular furnace in a H2 / Ar atmosphere, maintained at 250°C for 2 hours, and then naturally cooled to room temperature to obtain a catalyst.

[0076] 100 mg of the obtained catalyst was loaded onto a fixed bed, the flow rates of N2 and H2 were set to 15 mL / min and 45 mL / min, respectively, and a xenon lamp was turned on to test the activity of the catalyst in photothermal synthesis of ammonia under illumination.

[0077] The experimental results are as follows:

[0078] The photothermal activity of Ru-Al2O3-LaB6 under light irradiation was tested to be 237 μmol g -1 h -1 .

Claims

1. A method for preparing a supported rare earth hexaboride nanomaterial, characterized in that: The following steps are involved: (1) weighing a rare earth precursor, a boron precursor and a reducing agent in sequence according to a certain stoichiometric ratio, using zirconium oxide balls as grinding media, and then placing them in a grinding jar; (2) placing the sample-filled grinding jar in a planetary ball mill for ball milling at a speed of 400-600 r / min and a ball milling time of 15-60 h; (3) The ball-milled product is washed with alkaline solution and deionized water in sequence, and then dried to obtain a supported rare earth hexaboride nanomaterial.

2. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (1): the rare earth element type contained in the rare earth precursor includes but is not limited to one of La, Ce, Pr, Nd, Sm or Eu.

3. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (1): the rare earth precursor includes but is not limited to one or more of rare earth oxides, rare earth hydroxides, rare earth carbonates, and rare earth oxalates.

4. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (1): the boron precursor includes but is not limited to one or more of boron trioxide, elemental boron powder, sodium borohydride / potassium borohydride, and sodium metaborate.

5. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (1): the reducing agent is Al powder.

6. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (1): the molar ratio of the rare earth atom, the boron atom and the reducing agent is 1:6:7-15.

7. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (1), the grinding medium is a zirconia ball with a diameter of 5-10 mm, and the ball-to-material mass ratio is 5-10:

1.

8. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (2): the ball milling is carried out under a protective atmosphere, and the protective atmosphere is argon.

9. The method for preparing a supported rare earth hexaboride nanomaterial according to claim 1, characterized in that: In step (3), the alkali solution is an aqueous solution of sodium hydroxide with a concentration of 1-3 mol / L, the drying temperature is 70° C., and the drying time is 8 h.

10. Use of a supported rare earth hexaboride nanomaterial prepared by the method of any one of claims 1 to 9 as a catalyst carrier for photothermal ammonia synthesis reaction.

Citation Information

Patent Citations

  • Method for preparing LaB6 nano-powder through mechanical alloying process

    CN102225771A

  • Method for preparing rare earth metal hexaboride through aluminothermic reduction

    CN113772711A

  • General synthesis of metal borides in liquid salt melts

    EP2423164A1

  • Preparation of rare earth borides

    US4999176A