Method for preparing flaky low-sodium alpha-aluminum oxide by utilizing secondary aluminum ash
Through high-temperature sintering method and pickling and washing treatment, combined with additives and dilute alkali liquid treatment, the problem of low alumina purity in secondary aluminum ash was solved, and high-purity low-sodium flake α-alumina was prepared, reducing costs and avoiding Contamination is suitable for a variety of high-end applications.
Patent Information
- Application Number
- CN202410886731.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-03
AI Technical Summary
In the prior art, the alumina extracted from secondary aluminum ash has a low purity, and the preparation of sheet alumina is high cost, low efficiency, and serious pollution, making it difficult to achieve low sodium sheet alumina with high purity and low sodium content. Aluminum preparation.
High-temperature sintering combined with pickling and water washing treatment, by adding additives such as sodium carbonate, oxidizing agent and calcium carbonate to react with secondary aluminum ash, deeply desilicate and remove harmful elements, and use dilute alkali liquid and aluminum hydroxide seeds for crystallization and Calcination, and finally, by pickling and water washing, obtaining high-purity flake low-sodium alpha-alumina.
It has achieved high purity and low sodium content of sheet-shaped low-sodium α-alumina preparation, which is low-cost, suitable for industrial production, and avoids environmental pollution and equipment corrosion. It is suitable for high-end automobile polishing, gem processing and other fields.
Smart Images

Figure CN118978175A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary aluminum ash recovery and alpha-alumina preparation, and specifically relates to a method for preparing flaky low-sodium alpha-alumina by utilizing secondary aluminum ash. Background Art
[0002] With the rapid development of my country's economy, the demand for aluminum continues to increase, and my country has become the world's largest aluminum producer. With the continuous expansion of the production scale of aluminum and aluminum alloys in my country, the production of secondary aluminum slag has also shown a sharp growth trend. Secondary aluminum slag is the product of the slag produced in the production process of electrolytic aluminum or cast aluminum after cooling and processing. It is a recyclable resource. Generally, 30 to 50 kg of secondary aluminum slag is produced for every ton of aluminum produced. Its main components are Al, Al2O3, Fe, SiO2, nitrides, metal oxides, etc., among which Al and Al2O3 with the highest content can reach 10 to 80 wt%. The main component of secondary aluminum slag is aluminum oxide, which is a stable oxide of aluminum and a high hardness compound with a high melting point and boiling point. It is also called alumina in mining, ceramics and materials science. It can be used as an analytical reagent, dehydration of organic solvents, adsorbent, organic reaction catalyst, abrasive, polishing agent and refractory material, etc., so it has a wide range of uses.
[0003] Since the content of Al2O3 in secondary aluminum ash is high and secondary aluminum ash is a toxic and hazardous substance, direct disposal will damage the environment. According to the "National List of Hazardous Wastes" (2016), the four types of waste slags, namely, waste slag generated by the maintenance and disposal of electrolytic cells during aluminum electrolysis, primary smelting slag generated during aluminum pyrometallurgy, salt slag and slag generated during aluminum electrolysis, and flammable skimming slag generated during aluminum pyrometallurgy, belong to HW48 non-ferrous metal smelting waste. Therefore, extracting alumina from secondary aluminum ash not only realizes the resource utilization of secondary aluminum ash, but also promotes environmentally friendly development. However, since secondary aluminum ash contains a variety of impurities, in the prior art, the purity of alumina extracted from secondary aluminum ash is relatively low. How to obtain high-purity alumina has become a common pursuit of scientific researchers, and it also has extremely high economic and social significance.
[0004] Low-sodium flake α-alumina not only has the excellent properties of conventional α-alumina such as high hardness, high melting point, high temperature resistance, corrosion resistance, and good thermal conductivity, but also its special two-dimensional planar structure gives it special properties such as good adhesion, significant shielding effect and the ability to reflect light. It has great application potential in high-end automotive polishing, gemstone processing and high-precision microelectronics processing, cosmetics, functional coatings and ceramic toughening.
[0005] Therefore, using secondary aluminum ash as raw material to prepare low-sodium flaky α-alumina can not only realize the resource utilization of secondary aluminum ash slag, but also is environmentally friendly. It can also prepare high-quality low-sodium flaky α-alumina products, and has very good application prospects. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing flaky low-sodium α-alumina using secondary aluminum ash. This method is not only a new method for comprehensive utilization of secondary aluminum ash, but also eliminates the pollution problem of ammonia gas generated by incomplete denitrification of aluminum ash for aluminum nitride in aluminum ash and a large amount of fluoride in electrolytic refining, and achieves the removal of harmful elements in aluminum ash to achieve the purpose of harmless treatment and resource utilization. Moreover, this method is also a new method for preparing flaky low-sodium α-alumina, which uses a high-temperature sintering method to prepare aluminum oxide, improves the performance of the product by acid washing or water washing, and overcomes the shortcomings of high cost, low efficiency, low purity, and serious pollution of the prior art for preparing flaky aluminum oxide. The obtained low-sodium flaky low-sodium α-alumina has the advantages of perfect crystal development, high purity, low sodium content, high content of α-alumina, and micro-nano particle size. It has great application potential in the fields of high-end automobile polishing, gem processing and high-precision microelectronics processing, cosmetics, functional coatings and ceramic toughening.
[0007] A method for preparing flaky low-sodium α-alumina using secondary aluminum ash specifically comprises the following steps:
[0008] (1) crushing and grinding the secondary aluminum ash and sieving it;
[0009] (2) mixing the aluminum ash crushed and ground in step (1) with an additive and then roasting; the additive is a mixture of sodium carbonate, an oxidant, and calcium carbonate; the oxidant includes at least one of sodium nitrate, sodium percarbonate, sodium peroxide, and calcium peroxide;
[0010] (3) taking out the clinker roasted in step (2), cooling it, dissolving it with a dilute alkali solution or water, separating the solid from the liquid, and obtaining a filtrate which is a crude sodium aluminate solution;
[0011] (4) adding calcium oxide to deeply desiliconize the crude sodium aluminate solution, adding aluminum hydroxide seed crystals to crystallize to obtain aluminum hydroxide, filtering the aluminum hydroxide and then calcining it at high temperature to obtain aluminum oxide;
[0012] (5) The alumina obtained in step (4) is pickled and washed with water, and then dried to obtain flaky low-sodium α-alumina.
[0013] Step (1) Pass through a 200-mesh sieve.
[0014] In step (2), the amount of sodium carbonate added is 1.4-3 times the amount of aluminum oxide in the secondary aluminum ash, the amount of oxidant added is 1.2-2.4 times the amount of aluminum nitride in the secondary aluminum ash; and the amount of calcium carbonate added is 2.6-4.6 times the total amount of fluoride and silicon dioxide in the secondary aluminum ash.
[0015] The calcination temperature of step (2) is 800-1300° C. and the calcination time is 1-5 h.
[0016] In step (2), the additive reacts with the metal in the secondary aluminum ash at a high temperature to obtain a corresponding carbonate precipitate.
[0017] The dilute alkali solution used in step (3) includes: sodium carbonate solution or sodium hydroxide solution, with a concentration of 1-3 mol / L and a dissolution time of at least 30 minutes.
[0018] The insoluble filter residue after filtering in step (3) is fluorine-containing residue, which is returned to the electrolytic cell for use.
[0019] In step (4), the dosage ratio of calcium oxide is 10-30g / 500g secondary aluminum ash, and the addition amount of aluminum hydroxide seeds is 250-350g aluminum hydroxide seeds / 500g secondary aluminum ash; and then high-temperature calcination is performed to obtain aluminum oxide.
[0020] Step (4) calcination treatment, the temperature is set to 1000-1400°C, the time is set to 2-5h, and the rate is controlled at 5-10°C / min.
[0021] Step (3) mainly involves the reaction of alkali solution with all metals to generate a precipitate, which is separated to obtain a crude sodium aluminate solution. In step (4), the crude sodium aluminate solution is separated and purified, and then seed aluminum hydroxide is added to obtain aluminum hydroxide, which is then calcined at high temperature to obtain aluminum oxide.
[0022]
[0023] In step (5), the type of acid includes one or more of nitric acid, carbonic acid, acetic acid, oxalic acid, hydrochloric acid or citric acid; the concentration of the acid is controlled in the range of 0.03%-3.0%, and the solid content of the slurry is controlled to be 20-60% during pickling; the pickling time is controlled to be 1-5h during pickling; the pH value of the slurry is controlled to be 6.0-8.0; after pickling, the slurry is washed with pure water or ultrapure water until it is neutral, and dried at a temperature of 60°C-110°C for at least 6h.
[0024] The sodium oxide content of the flaky low-sodium α-alumina obtained by the present invention can be as low as 0.13%, and the particle size is 20-50 microns. The flaky low-sodium α-alumina prepared by the present invention has good stability, a simple preparation process, low cost, and is suitable for industrial production. The present invention can control the density and fluidity of the slurry by controlling the solid content of the slurry at 20-60% during the pickling process, which is convenient for industrial production and washing and removing sodium oxide; by controlling the pH value to about 7.0 during the pickling and water washing processes, the sodium oxide content after pickling can be controlled and reduced to avoid pollution to the environment and damage to the equipment. Compared with the prior art, the present invention does not need to introduce salt sphering liquid or additives with a de-sodium effect, and directly uses pure water or softened water, which effectively avoids corrosion to the pipeline. The process operation is simple, the cost is low, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the secondary aluminum ash raw material diagram;
[0026] Figure 2 It is the flake α-Al2O3 product prepared by the present invention;
[0027] Figure 3 This is the SEM image of the original sample of secondary aluminum ash;
[0028] Figure 4 This is a SEM image of the flaky α-Al2O3 prepared by the present invention;
[0029] Figure 5 This is the XRD pattern of the secondary aluminum ash as is;
[0030] Figure 6 This is the XRD diagram of the flaky α-Al2O3 prepared by the present invention. DETAILED DESCRIPTION
[0031] The following examples are intended to further illustrate the present invention, but are not intended to limit the present invention.
[0032] Example 1
[0033] A method for preparing flaky low-sodium α-alumina using secondary aluminum ash, the specific steps are as follows:
[0034] (1) The secondary aluminum ash is crushed and sieved with a crusher (200 mesh, 500 g);
[0035] (2) mixing the crushed and ground aluminum ash obtained in step (1) with the additives and then calcining the mixture (temperature: 1200° C., time: 3 h), and recovering the sintering gas;
[0036] (3) The clinker after roasting in step (2) is taken out and cooled to room temperature, and then dissolved with a dilute alkali solution (1M sodium hydroxide solution for 1 hour, solid-liquid separation, the filtrate is a crude sodium aluminate solution, and the insoluble filter residue is a fluorine-containing residue that is returned to the electrolytic cell for use; calcium oxide (calcium oxide addition amount 10g) is added to the crude sodium aluminate solution, and the sodium aluminate solution after deep desiliconization is decomposed by seed crystals (aluminum hydroxide seed crystal addition amount 200g) to obtain aluminum hydroxide, and then high-temperature calcination (temperature 1400°C, time 5h, heating rate 5°C / min) to obtain aluminum oxide;
[0037] (4) The alumina product obtained in step (3) is pickled (with citric acid), and the acid concentration is controlled at 0.03%; the solid content of the slurry is controlled to 40% during pickling; the pickling time is controlled to 2 hours during pickling; the pH value of the slurry is controlled to 7.0; the pickled slurry is washed with pure water or ultrapure water (washed to a pH value of 7.0), and dried (temperature controlled at 100°C, drying for 6 hours). The sodium oxide content of the flaky low-sodium α-alumina obtained after pickling and washing is controlled to be as low as 0.13%.
[0038] The additive in step (2) is a mixture of sodium carbonate, an oxidant and calcium carbonate; the oxidant is sodium nitrate, the amount of sodium carbonate added is twice the amount of aluminum oxide in the aluminum ash, the amount of the oxidant added is 2.4 times the amount of aluminum nitride in the aluminum ash; and the amount of calcium carbonate added is three times the total amount of fluoride and silicon dioxide in the aluminum ash.
[0039] The secondary aluminum ash is used as raw material, and its index parameter percentage content is:
[0040]
[0041] The flaky low-sodium α-alumina obtained by the method of the present invention has the following index parameter percentage content:
[0042]
[0043] Example 2
[0044] All steps were the same as in Example 1, except that the concentration of citric acid was 1%.
[0045] The flaky low-sodium α-alumina obtained by the method of the present invention has the following index parameter percentage content:
[0046]
[0047] Example 3
[0048] All steps were the same as in Example 1, except that the concentration of citric acid was 3%.
[0049] The flaky low-sodium α-alumina obtained by the method of the present invention has the following index parameter percentage content:
[0050]
[0051] Under the premise that the other conditions are the same as those in Example 1, the present invention finds that the type and concentration of the acid during pickling have a greater impact on the performance parameters of the final product. The specific comparison results are as follows:
[0052] Different types of acids:
[0053]
[0054] Different citric acid concentrations:
[0055]
Claims
1. A method for preparing flaky low-sodium α-alumina using secondary aluminum ash, characterized in that: The specific steps include: (1) crushing and grinding the secondary aluminum ash and sieving it; (2) mixing the aluminum ash crushed and ground in step (1) with an additive and then roasting; the additive is a mixture of sodium carbonate, an oxidant, and calcium carbonate; the oxidant includes at least one of sodium nitrate, sodium percarbonate, sodium peroxide, and calcium peroxide; (3) taking out the clinker roasted in step (2), cooling it, dissolving it with a dilute alkali solution or water, separating the solid from the liquid, and obtaining a filtrate which is a crude sodium aluminate solution; (4) adding calcium oxide to deeply desiliconize the crude sodium aluminate solution, adding aluminum hydroxide seed crystals to crystallize to obtain aluminum hydroxide, filtering the aluminum hydroxide and then calcining it at high temperature to obtain aluminum oxide; (5) The alumina obtained in step (4) is pickled and washed with water, and then dried to obtain flaky low-sodium α-alumina.
2. The preparation method according to claim 1, characterized in that: Step (1) Pass through a 200-mesh sieve.
3. The preparation method according to claim 1, characterized in that: In step (2), the amount of sodium carbonate added is 1.4-3 times the amount of aluminum oxide in the secondary aluminum ash, the amount of oxidant added is 1.2-2.4 times the amount of aluminum nitride in the secondary aluminum ash; and the amount of calcium carbonate added is 2.6-4.6 times the total amount of fluoride and silicon dioxide in the secondary aluminum ash.
4. The preparation method according to claim 1 or 3, characterized in that: The calcination temperature of step (2) is 800-1300° C. and the calcination time is 1-5 h.
5. The preparation method according to claim 1, characterized in that: The dilute alkali solution used in step (3) includes: sodium carbonate solution or sodium hydroxide solution, with a concentration of 1-3 mol / L and a dissolution time of at least 30 minutes.
6. The preparation method according to claim 1 or 5, characterized in that: The insoluble filter residue after filtering in step (3) is fluorine-containing residue, which is returned to the electrolytic cell for use.
7. The preparation method according to claim 1, characterized in that: In step (4), the dosage ratio of calcium oxide is 10-30g / 500g secondary aluminum ash, and the addition amount of aluminum hydroxide seeds is 250-350g aluminum hydroxide seeds / 500g secondary aluminum ash; and then high-temperature calcination is performed to obtain aluminum oxide.
8. The preparation method according to claim 1 or 7, characterized in that: Step (4) calcination treatment, the temperature is set to 1000-1400°C, the time is set to 2-5h, and the rate is controlled at 5-10°C / min.
9. The preparation method according to claim 1, characterized in that: In step (5), the type of acid includes one or more of nitric acid, carbonic acid, acetic acid, oxalic acid, hydrochloric acid or citric acid; the concentration of the acid is controlled in the range of 0.03%-3.0%, and the solid content of the slurry is controlled to be 20-60% during pickling; the pickling time is controlled to be 1-5h during pickling; the pH value of the slurry is controlled to be 6.0-8.0; after pickling, the slurry is washed with pure water or ultrapure water until it is neutral, and dried at a temperature of 60°C-110°C for at least 6h.
10. The preparation method according to claim 1 or 9, characterized in that: The sodium oxide content of the obtained flaky low-sodium α-alumina is not more than 0.13%.
Citation Information
Patent Citations
Comprehensive utilization method of secondary aluminum ash
CN112279283A
Preparation process of ultralow-sodium aluminum oxide and ultralow-sodium aluminum oxide
CN112850761A
Preparation method of low-sodium and ultralow-sodium tabular sintered corundum
CN115073147A
Preparation of low-soda alumina
KR1020040041236A
Cited By
Method for rapid detoxification and resource utilization of secondary aluminum ash
CN119976911A
High-value utilization method of calcium carbide slag cooperating with secondary aluminum ash
CN121757900A