Metal alkoxide modified nickel-iron-manganese-zinc sodium quaternary positive electrode material, preparation method thereof and sodium ion battery
Through element doping and surface chemical modification technology, spherical sodium nickel ferromanganic acid cathode material with high specific capacity and high stability was prepared, solving the problems of high diffusion energy barrier and complex phase transition in sodium ion batteries. , significantly improves the cycle life and electrochemical performance of the battery.
Patent Information
- Application Number
- CN202411076469.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
During the charging and discharging process, the existing sodium ion battery positive electrode materials have high diffusion energy barrier and complex phase transition, resulting in limited capacity attenuation and cycle life, and the distortion of the transition metal layer affects the battery performance.
The spherical sodium ferromanganate positive electrode material was prepared by element doping and surface chemical modification. Through co-precipitation, ball milling, sintering, ultrasonic dispersion and heat treatment, the metal alkoxide modified sodium ferromanganate was formed. The cathode material enhances the stability and electrochemical properties of the material.
The stability and cycle life of the cathode material were improved. The first Coulomb efficiency reached 93.38%, and the cycle stability of the battery was significantly improved within the 2-4.0V voltage range, which was 5% higher than that of the unmodified cathode material.
Smart Images

Figure CN118978194A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and in particular relates to a metal alkoxide-modified sodium nickel-iron-manganese-zincate quaternary positive electrode material, a preparation method thereof, and a sodium ion battery. Background Art
[0002] With the continuous development of the battery industry, sodium-ion batteries have attracted widespread attention and research due to their advantages of abundant resources, environmental friendliness and high energy density.
[0003] Among various types of sodium ion cathode materials, the Na a Ni x Fe y Mn z M 1-x-y-z O2 (M = Mg, Ti, Fe, Co, Ni, Cu, Zn, V, etc.) is used as a positive electrode material, a layered oxide, which has a high theoretical capacity, is easy to prepare and is environmentally friendly. O3-type materials have the outstanding advantages of high sodium ion content, large voltage window, and high energy density. However, the sodium ions in O3 materials have a high migration and diffusion energy barrier, facing the complex phase transitions that occur during the sodium ion deintercalation process and the distortion of the transition metal layer during the charge and discharge process, which will cause the capacity of the layered positive electrode material to decay. Due to the phase change of the material to produce a spinel phase or a rock salt phase, the process is accompanied by the release of lattice oxygen. As a result, the battery capacity and cycle life of the sodium ion battery are greatly affected.
[0004] Therefore, there is an urgent need to develop a sodium ion battery positive electrode material with high stability and excellent battery performance. Summary of the invention
[0005] In order to overcome the problems in the prior art, the present invention prepares a modified positive electrode material by element doping and surface chemical modification to improve the stability of the positive electrode material and further increase the capacity and cycle life of the sodium ion battery.
[0006] In an embodiment of the present invention, the present invention provides a method for preparing a spherical nickel iron manganese zincate positive electrode material with high specific capacity and high stability, the method comprising the following steps:
[0007] S1. Dissolving nickel salt, iron salt, manganese salt and zinc salt in a stoichiometric ratio in deionized water to prepare a metal salt solution, adding a precipitant and a complexing agent under an inert atmosphere, adjusting the pH value to perform a coprecipitation reaction to obtain a hydroxide precursor;
[0008] S2, ball-milling the hydroxide precursor and the sodium source, and then sintering at high temperature in an oxidizing atmosphere to obtain a sodium nickel iron manganese zincate positive electrode material;
[0009] S3, adding the metal alkoxide to the ethanol solution, stirring and dissolving to obtain a mixed solution;
[0010] S4, adding the sodium nickel iron manganese zincate positive electrode material to the mixed solution, performing ultrasonic dispersion under sealing conditions, and then performing vacuum drying to obtain a positive electrode material pretreated with a metal alkoxide;
[0011] S5. Heat-treating the positive electrode material pretreated with metal alkoxide to obtain a metal alkoxide-modified sodium nickel-iron-manganese-zinc quaternary positive electrode material.
[0012] In a specific embodiment of the invention, the metal alkoxide is any one or more of the metal alkoxides of Nb, Ta, Mo, Mg, Al, Ca, Zr, Ti, and V.
[0013] In a specific embodiment of the invention, in step S1, the nickel salt, iron salt, manganese salt and zinc salt are one or more of soluble sulfates, nitrates, formates and acetates, the precipitant is a sodium hydroxide solution with a concentration of 2 to 6 mol / L; the complexing agent is an ammonia solution with a concentration of 10 to 40 wt%, the pH value is 10 to 12, and the coprecipitation reaction time is 10 to 30 h.
[0014] In a specific embodiment of the invention, in step S2, the sodium salt is one or more of sodium carbonate, sodium hydroxide, sodium acetate, sodium nitrate, sodium formate and sodium iodide.
[0015] In a specific embodiment of the invention, in step S2, the high-temperature sintering process includes pre-calcination and high-temperature calcination, the pre-calcination is to increase the temperature from room temperature to 300-600°C at a heating rate of 1-10°C / min, and the pre-calcination time is 4-10h; the high-temperature calcination is to increase the temperature to 800-1000°C at a heating rate of 1-10°C / min, and the calcination time is 6-15h; the oxygen content in the oxidizing atmosphere exceeds 50%, and the water and CO2 contents are less than 0.1%.
[0016] In a specific embodiment of the invention, the molar ratio of transition metal ions to metal alkoxides in the positive electrode material is 1:0.0002-0.03.
[0017] In a specific embodiment of the invention, in step S5, the heat treatment temperature is 400-800° C., and the treatment time is 3-6 hours.
[0018] Based on the same inventive concept, there is also provided a metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material prepared by the above-mentioned preparation method, wherein the chemical formula of the positive electrode material is M@Na a Ni x Fe y Mn z Zn 1-x-y-zO2, wherein 0.8≤a≤1.05, 0≤x≤1 / 3, 0≤y≤1 / 3, 0≤z≤1 / 3, and M is one or more of Nb, Ta, Mo, Mg, Al, Ca, Zr, Ti, and V.
[0019] In a specific embodiment, the primary particles of the positive electrode material are in the form of flakes with a size of 100 to 200 nm, and the secondary particles are in the form of porous spherical structures with a size of 4 to 10 μm.
[0020] The present invention also provides a sodium ion battery, which comprises the above-mentioned metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention uses a high-solubility metal alkoxide to modify the positive electrode material. The positive electrode material is ultrasonically dispersed in an ethanol solution of the metal alkoxide, and the modified positive electrode material is obtained by drying and high-temperature calcination. In this process, ethanol is used as a solvent. On the one hand, the great influence of moisture on the layered oxide positive electrode material of the sodium ion battery can be avoided. On the other hand, ethanol can increase the solubility of the metal alkoxide. The positive electrode material prepared by this method has a good morphology. The temperature of the high-temperature calcination can be controlled to achieve a controllable doping depth and improve the stability of the positive electrode material.
[0023] (2) The metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material provided by the present invention is doped with metal ions on the surface, and a stronger TM-O bond can be formed on the surface of the material, so that the surface oxygen is inactivated, the TM-O hybridization of the surface appendages is reduced, and the structure is stable; when applied to sodium ion batteries, the stability is significantly improved. In the voltage range of 2-4.0V, the first coulomb efficiency is 93.38%, and its cycle stability is improved by 5% compared with the unmodified positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 XRD diagram of the sodium nickel iron manganese zincate positive electrode material prepared in Example 1 and Comparative Example 1;
[0026] Figure 2 This is a SEM image of the metal alkoxide-modified sodium nickel iron manganese zincate positive electrode material prepared in Example 1;
[0027] Figure 3The internal morphology and Nb element distribution diagram of the metal alkoxide-modified sodium nickel iron manganese zincate positive electrode material prepared in Example 1 after argon ion cutting;
[0028] Figure 4 The metal alkoxide-modified Na prepared in Example 1 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 The first charge and discharge curve of the button cell assembled with O2 positive electrode material at a discharge rate of 0.1C;
[0029] Figure 5 The Na prepared in Examples 1, 2, 3 and Comparative Example 1 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 Electrochemical performance of button cells assembled with O2 materials at 1C discharge rate;
[0030] Figure 6 The Na prepared in Examples 4, 5 and Comparative Example 1 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 Electrochemical performance of button cells assembled with O2 materials at 1C discharge rate. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0032] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0034] In order to improve the electrical properties of the positive electrode material, the present invention provides a method for preparing a spherical nickel iron manganese zincate positive electrode material with high specific capacity and high stability, the method comprising the following steps:
[0035] S1. Dissolve nickel salt, iron salt, manganese salt and zinc salt in deionized water in a stoichiometric ratio to prepare a metal salt solution, add a precipitant and a complexing agent under an inert atmosphere, adjust the pH value to 10-12, perform a coprecipitation reaction for 10-30 hours, and obtain a hydroxide precursor by suction filtration, washing, impurity removal and drying. In this process, the nickel salt, iron salt, manganese salt and zinc salt are one or more soluble sulfates, nitrates, formates and acetates, the precipitant is a sodium hydroxide solution with a concentration of 2-6 mol / L; the complexing agent is an ammonia solution with a concentration of 10-40wt%.
[0036] S2. After ball-milling and mixing the hydroxide precursor and the sodium source, high-temperature sintering is performed in an oxidizing atmosphere to obtain a sodium nickel iron manganese zincate positive electrode material; wherein the sodium source is one or more of sodium carbonate, sodium hydroxide, sodium acetate, sodium nitrate, sodium formate and sodium iodide. The high-temperature sintering of this process includes pre-calcination and high-temperature calcination, wherein the pre-calcination is heated from room temperature to 300-600°C at a heating rate of 1-10°C / min, and the pre-calcination is 4-10h; the high-temperature calcination is heated to 800-1000°C at a heating rate of 1-10°C / min, and the calcination time is 6-15h; and the oxidizing environment is: the oxygen content exceeds 50%, and the water and CO2 contents are less than 0.1%.
[0037] S3. Add any one or more metal alkoxides such as Nb, Ta, Mo, Mg, Al, Ca, Zr, Ti, and V to an ethanol solution with a concentration of more than 95% (preferably 99.7%), and stir to dissolve to obtain a mixed solution; wherein the amount of the metal alkoxide added is calculated according to the molar ratio of transition metal ion to metal alkoxide of 1:0.0002 to 0.03.
[0038] S4, adding the sodium nickel iron manganese zincate positive electrode material to the mixed solution, performing ultrasonic dispersion for 50 to 80 minutes under a sealed condition, and then performing vacuum drying for 10 to 15 hours at a temperature of 50 to 70° C. to obtain a positive electrode material pretreated with a metal alkoxide;
[0039] S5. Heat-treating the positive electrode material pretreated with metal alkoxide at a temperature of 400-800° C. for 3-6 hours to obtain a metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material.
[0040] Based on the same inventive concept, there is also provided a metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material prepared by the above-mentioned preparation method, whose chemical formula is M@Na a Ni x Fe y Mn z Zn 1-x-y-zO2, wherein 0.8≤a≤1.05, 0≤x≤1 / 3, 0≤y≤1 / 3, 0≤z≤1 / 3, and M is one or more of Nb, Ta, Mo, Mg, Al, Ca, Zr, Ti, and V. The primary particles of the positive electrode material are 100-200 nm flakes, and the secondary particles are 4-10 μm porous spherical structures.
[0041] The present invention also provides a sodium ion battery, which comprises the above-mentioned metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material.
[0042] The above introduces the specific implementation methods of the present application. In order to objectively illustrate the technical effects produced by the present application, the following examples and comparative examples will be used for description.
[0043] Example 1
[0044] A metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material and a preparation method thereof comprises the following steps:
[0045] NiSO4·7H2O, FeSO4·7H2O, MnSO4·H2O and ZnSO4·7H2O were dissolved in deionized water at a molar ratio of 0.27:0.33:0.33:0.06 to prepare a 2 mol / L metal ion solution, which was then added to a continuous stirred tank reactor under nitrogen atmosphere protection, and after adding 4 mol / L NaOH precipitant and 20 wt% NH3·H2O complexing agent, the pH of the solution was maintained in the range of 10-11. After sufficient reaction, the solution was filtered, washed repeatedly, impurities were removed, and dried to obtain Ni 1 / 15 Fe 1 / 3Mn 1 / 3 Zn 4 / 15 OH precursor. Take 1 mol Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 The OH precursor was fully ball-milled with 0.900 mol Na2CO3, heated to 500°C at 5°C / min in an atmosphere furnace, pre-sintered for 4 h, and then heated to 890°C and sintered for 12 h to obtain Na 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 O2 positive electrode material. Take 0.004 mol of niobium ethoxide and mix it with 99.7% ethanol solution to obtain mixed solution 1. Add the positive electrode material to mixed solution 1, ultrasonically disperse it for 60 minutes, and vacuum dry it at 60°C for 12 hours to obtain the positive electrode material pretreated with niobium ethoxide. Then, anneal it at 600°C for 4 hours to obtain the target positive electrode material.
[0046] Example 2
[0047] A metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material and a preparation method thereof, comprising the following steps:
[0048] NiSO4·7H2O, FeSO4·7H2O, MnSO4·H2O and ZnSO4·7H2O were dissolved in deionized water at a molar ratio of 0.27:0.33:0.33:0.06 to prepare a 2 mol / L metal ion solution, which was then added to a continuous stirred tank reactor under nitrogen atmosphere protection, and after adding 4 mol / L NaOH precipitant and 20 wt% NH3·H2O complexing agent, the pH of the solution was maintained in the range of 10-11. After sufficient reaction, the solution was filtered, washed repeatedly, impurities were removed, and dried to obtain Ni 1 / 15 Fe 1 / 3Mn 1 / 3 Zn 4 / 15 OH precursor. Take 1 mol Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 The OH precursor was fully ball-milled with 0.900 mol Na2CO3, heated to 500°C at 5°C / min in an atmosphere furnace, pre-sintered for 4 h, and then heated to 890°C and sintered for 12 h to obtain Na 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 O2 positive electrode material. Take 0.004 mol of niobium ethoxide and mix it with 99.7% ethanol solution to obtain mixed solution 1. Add the positive electrode material to mixed solution 1, ultrasonically disperse for 60 minutes, and vacuum dry at 60°C for 12 hours to obtain the positive electrode material pretreated with niobium ethoxide. Then, anneal at 500°C for 4 hours to obtain the target positive electrode material.
[0049] Example 3
[0050] A metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material and a preparation method thereof, comprising the following steps:
[0051] NiSO4·7H2O, FeSO4·7H2O, MnSO4·H2O and ZnSO4·7H2O were dissolved in deionized water at a molar ratio of 0.27:0.33:0.33:0.06 to prepare a 2 mol / L metal ion solution, which was then added to a continuous stirred tank reactor under nitrogen atmosphere protection, and after adding 4 mol / L NaOH precipitant and 20 wt% NH3·H2O complexing agent, the pH of the solution was maintained in the range of 10-11. After sufficient reaction, the solution was filtered, washed repeatedly, impurities were removed, and dried to obtain Ni 1 / 15 Fe 1 / 3Mn 1 / 3 Zn 4 / 15 OH precursor. Take 1 mol Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 The OH precursor was fully ball-milled with 0.900 mol Na2CO3, heated to 500°C at 5°C / min in an atmosphere furnace, pre-sintered for 4 h, and then heated to 890°C and sintered for 12 h to obtain Na 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 O2 positive electrode material. Take 0.004 mol of niobium ethoxide and mix it with 99.7% ethanol solution to obtain mixed solution 1. Add the positive electrode material to mixed solution 1, ultrasonically disperse it for 60 minutes, and vacuum dry it at 60°C for 12 hours to obtain the positive electrode material pretreated with niobium ethoxide. Then, anneal it at 800°C for 4 hours to obtain the target positive electrode material.
[0052] Example 4
[0053] A metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material and a preparation method thereof, comprising the following steps:
[0054] NiSO4·7H2O, FeSO4·7H2O, MnSO4·H2O and ZnSO4·7H2O were dissolved in deionized water at a molar ratio of 0.27:0.33:0.33:0.06 to prepare a 2 mol / L metal ion solution, which was then added to a continuous stirred tank reactor under nitrogen atmosphere protection, and after adding 4 mol / L NaOH precipitant and 20 wt% NH3·H2O complexing agent, the pH of the solution was maintained in the range of 10-11. After sufficient reaction, the solution was filtered, washed repeatedly, impurities were removed, and dried to obtain Ni 1 / 15 Fe 1 / 3Mn 1 / 3 Zn 4 / 15 OH precursor. Take 1 mol Ni 1 / 15 Fe1 / 3 Mn 1 / 3 Zn 4 / 15 The OH precursor was fully ball-milled with 0.900 mol Na2CO3, heated to 500°C at 5°C / min in an atmosphere furnace, pre-sintered for 4 h, and then heated to 890°C and sintered for 12 h to obtain Na 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 O2 positive electrode material. Take 0.005 mol of tantalum ethoxide and mix it with 99.7% ethanol solution to obtain mixed solution 1. Add the positive electrode material to mixed solution 1, ultrasonically disperse for 60 minutes, and vacuum dry at 60°C for 12 hours to obtain the positive electrode material pretreated with tantalum ethoxide. Then, anneal at 600°C for 4 hours to obtain the target positive electrode material.
[0055] Example 5
[0056] A metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material and a preparation method thereof, comprising the following steps:
[0057] NiSO4·7H2O, FeSO4·7H2O, MnSO4·H2O and ZnSO4·7H2O were dissolved in deionized water at a molar ratio of 0.27:0.33:0.33:0.06 to prepare a 2 mol / L metal ion solution, which was then added to a continuous stirred tank reactor under nitrogen atmosphere protection, and after adding 4 mol / L NaOH precipitant and 20 wt% NH3·H2O complexing agent, the pH of the solution was maintained in the range of 10-11. After sufficient reaction, the solution was filtered, washed repeatedly, impurities were removed, and dried to obtain Ni 1 / 15 Fe 1 / 3Mn 1 / 3 Zn 4 / 15 OH precursor. Take 1 mol Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 The OH precursor was fully ball-milled with 0.900 mol Na2CO3, heated to 500°C at 5°C / min in an atmosphere furnace, pre-sintered for 4 h, and then heated to 890°C and sintered for 12 h to obtain Na 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15O2 positive electrode material. Take 0.005 mol of zirconium isopropoxide and mix it with 99.7% ethanol solution to obtain mixed solution 1. Add the positive electrode material to mixed solution 1, ultrasonically disperse for 60 minutes, and vacuum dry at 60°C for 12 hours to obtain the positive electrode material pretreated with zirconium isopropoxide. Then, anneal at 600°C for 4 hours to obtain the target positive electrode material.
[0058] Comparative Example 1
[0059] A method for preparing a sodium nickel-iron-manganese-zincate quaternary positive electrode material comprises the following steps:
[0060] NiSO4·7H2O, FeSO4·7H2O, MnSO4·H2O and ZnSO4·7H2O were dissolved in deionized water at a molar ratio of 0.27:0.33:0.33:0.06 to prepare a 2 mol / L metal ion solution, which was then added to a continuous stirred tank reactor under nitrogen atmosphere protection, and after adding 4 mol / L NaOH precipitant and 20 wt% NH3·H2O complexing agent, the pH of the solution was maintained in the range of 10-11. After sufficient reaction, the solution was filtered, washed repeatedly, impurities were removed, and dried to obtain Ni 1 / 15 Fe 1 / 3Mn 1 / 3 Zn 4 / 15 OH precursor. Take 1 mol Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 The OH precursor was fully ball-milled with 0.900 mol Na2CO3, heated to 500°C at 5°C / min in an atmosphere furnace, pre-sintered for 4 h, and then heated to 890°C and sintered for 12 h to obtain Na 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 O2 positive electrode material.
[0061] Structural characterization and performance testing
[0062] The obtained positive electrode material was subjected to XRD analysis, scanning electron microscopy analysis, and internal morphology and element distribution analysis. The niobium-modified Na 0.9 Ni 1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 Taking O2 positive electrode material as an example, as shown in Figure (1), the material is an R-3m structure. Compared with comparative example 1, the characteristic peaks (003) and (104) of the material are shifted, indicating that Nb is successfully doped into the material surface. As shown in the SEM spectrum of Figure (2), niobium-modified Na 0.9 Ni1 / 15 Fe 1 / 3 Mn 1 / 3 Zn 4 / 15 O2 positive electrode material morphology, there are small particles on the surface of secondary particles, which may be niobium oxide attached or residual alkali on the surface of the material. As shown in the spectrum in Figure (3), it can be seen that the Nb content gradually decreases from the surface to the inside of the material.
[0063] The positive electrode materials obtained in Examples 1 to 5 and Comparative Example 1 were used as positive electrode materials for battery assembly to obtain sodium ion batteries and to perform performance tests. Battery assembly: Take 0.0800g of the above positive electrode material, add 0.0100g of conductive carbon black as a conductive agent and 0.0100g of PVDF (polyvinylidene fluoride) as a binder, mix well and apply it on aluminum foil to make a positive electrode sheet, and assemble into a CR2025 button cell in a vacuum glove box using a sodium sheet as the negative electrode, a Whatman GF / D glass fiber diaphragm as the battery separator, and 1 mol / L NaClO4 (EC:DMC=1:1 (volume ratio) + 5% FEC) as the electrolyte. After assembly, electrical performance tests were performed in the range of 2 to 4V. The test results are shown in Table 1 and Figure 4 , 5 , as shown in Figure 6.
[0064] Table 1 Electrical performance test results
[0065] Group Cathode Materials First Coulombic efficiency Discharge specific capacity Capacity retention rate Application Example 1 Example 1 93.38% 142.27mAh / g 70.79% Application Example 2 Example 2 96.05% 136.55mAh / g 70.4% Application Example 3 Example 3 99.71% 135.51mAh / g 67.6% Application Example 4 Example 4 89.25% 139.18mAh / g 70.05% Application Example 5 Example 5 90.04% 140.63mAh / g 74.34% Comparative application example 1 Comparative Example 1 91.35% 145.07mAh / g 65.4%
[0066] By comparing the above embodiments and comparative examples, it can be seen that the positive electrode material modified by metal alkoxide can improve the first coulombic efficiency of the material, but may sacrifice part of the discharge specific capacity, which is mainly due to the partial consumption of Na+ and H+ / H3O+ exchange when the material is immersed in ethanol solution; and the strong ionic TM-O bond is introduced into the sodium site or transition metal site, producing an oxygen anchoring effect, so that the surface oxygen oxidation is inhibited or delayed to a higher potential, reducing the migration of transition metals, thereby improving the cycle stability of the material.
[0067] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for preparing a metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material, characterized in that: The preparation method comprises the following steps: S1. Dissolving nickel salt, iron salt, manganese salt and zinc salt in a stoichiometric ratio in deionized water to prepare a metal salt solution, adding a precipitant and a complexing agent under an inert atmosphere, adjusting the pH value to perform a coprecipitation reaction to obtain a hydroxide precursor; S2, ball-milling the hydroxide precursor and the sodium source, and then sintering at high temperature in an oxidizing atmosphere to obtain a sodium nickel iron manganese zincate positive electrode material; S3, adding the metal alkoxide to the ethanol solution, stirring and dissolving to obtain a mixed solution; S4, adding the sodium nickel iron manganese zincate positive electrode material to the mixed solution, performing ultrasonic dispersion under sealing conditions, and then performing vacuum drying to obtain a positive electrode material pretreated with a metal alkoxide; S5. Heat-treating the positive electrode material pretreated with metal alkoxide to obtain a metal alkoxide-modified sodium nickel-iron-manganese-zinc quaternary positive electrode material.
2. The method for preparing the metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material according to claim 1, characterized in that: The metal alkoxide is any one or more of metal alkoxides of Nb, Ta, Mo, Mg, Al, Ca, Zr, Ti, and V.
3. The method for preparing the metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material according to claim 1, characterized in that: In step S1, the nickel salt, iron salt, manganese salt and zinc salt are one or more of soluble sulfates, nitrates, formates and acetates, the precipitant is a sodium hydroxide solution with a concentration of 2 to 6 mol / L; the complexing agent is an ammonia solution with a concentration of 10 to 40 wt%, the pH value is 10 to 12, and the coprecipitation reaction time is 10 to 30 hours.
4. The method for preparing the metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material according to claim 1, characterized in that: In step S2, the sodium salt is one or more of sodium carbonate, sodium hydroxide, sodium acetate, sodium nitrate, sodium formate and sodium iodide.
5. The method for preparing the metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material according to claim 1, characterized in that: In step S2, the high-temperature sintering process includes pre-calcination and high-temperature calcination. The pre-calcination is to increase the temperature from room temperature to 300-600°C at a heating rate of 1-10°C / min, and the pre-calcination is 4-10h; the high-temperature calcination is to increase the temperature to 800-1000°C at a heating rate of 1-10°C / min, and the calcination time is 6-15h; the oxygen content in the oxidizing atmosphere exceeds 50%, and the water and CO2 contents are less than 0.1%.
6. The method for preparing the metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material according to claim 1, characterized in that: The molar ratio of transition metal ions to metal alkoxide in the positive electrode material is 1:0.0002-0.
03.
7. The method for preparing the metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material according to claim 1, characterized in that: In the step S5, the heat treatment temperature is 400-800° C., and the treatment time is 3-6 hours.
8. The metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The chemical formula of the positive electrode material is M@Na a Ni x Fe y Mn z Zn 1-x-y-z O2, wherein 0.8≤a≤1.05, 0≤x≤1 / 3, 0≤y≤1 / 3, 0≤z≤1 / 3, and M is one or more of Nb, Ta, Mo, Mg, Al, Ca, Zr, Ti, and V.
9. The metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material according to claim 8, characterized in that: The primary particles of the positive electrode material are in the form of flakes with a size of 100 to 200 nm, and the secondary particles are in the form of porous spherical structures with a size of 4 to 10 μm.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the metal alkoxide-modified sodium nickel iron manganese zincate quaternary positive electrode material as described in any one of claims 8 to 9.