Method for recovering concentrated water in nanofiltration membrane section of lepidolite ore lithium extraction lixivium

By directly recovering fluorine ions and chloride ions in concentrated water in lithium mica extract leaching liquid in lithium mica ore, the cumbersome problems of recycling hydrofluoric acid and hydrogen chloride in the prior art are solved, and the cumbersome problems of recycling hydrofluoric acid and hydrogen chloride in the prior art are achieved. Efficient resource utilization.

CN118978210AActive Publication Date: 2024-11-19SHANTOU AOSBO ENVIRONMENTAL PROTECTION MATERIAL MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411043053.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

In the prior art, the recovery of concentrated water in the nanofiltration membrane section of lithium mica ore extract lithium leaching liquid in lithium, especially how to effectively recover fluorine ions and chloride ions to prepare hydrofluoric acid and hydrogen chloride has problems of cumbersome operations and complicated steps.

Method used

By gradually adding sulfuric acid to the concentrated water treated in the nanofiltration membrane section at different temperatures, multi-step treatment is carried out to remove chloride and fluorine ions, combined with the step-by-step addition and rehydration of sulfuric acid, the direct evaporation of hydrogen chloride and hydrofluoric acid can be achieved. and recycling.

Benefits of technology

The recycling and treatment of concentrated water sections is simplified to directly obtain hydrogen fluoride and hydrogen chloride, which is simple to operate and easy to obtain raw materials, achieving efficient recovery of fluoride and chloride ions in concentrated water, and providing a good strategy for resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978210A_ABST
    Figure CN118978210A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium extraction and wastewater recovery, and particularly discloses a method for recovering concentrated water in a nanofiltration membrane section of lepidolite ore lithium extraction leachate. The method comprises the following steps: 1) heating concentrated water collected after nanofiltration membrane section treatment at 90-100 DEG C, and evaporating to remove water; (2) adding sulfuric acid into the concentrated solution subjected to primary water removal in the step (1), heating at 110-120 DEG C, and evaporating to remove chloride ions; and 3) on the basis of the step 2), sulfuric acid is continuously added, heating is carried out at 150-160 DEG C, water is supplemented in the heating process, the dosage of the supplemented water is 25-30% of the mass of the concentrated water, and fluorine ions are removed through evaporation. According to the method, fluorine ions and chloride ions in the concentrated water section can be directly evaporated step by step to obtain a target object, secondary extraction and purification are not needed, raw materials are easy to obtain, operation is easy, simple recovery treatment can be conducted on the concentrated water section, meanwhile, corresponding products can be directly obtained in one step, and the method is suitable for industrial production. Therefore, a good treatment strategy for recycling the chloride ions and the fluorine ions in the concentrated water is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium extraction and wastewater recovery, and specifically discloses a method for recovering concentrated water from a nanofiltration membrane section of a lithium extraction leaching solution from a lepidolite mine. Background Art

[0002] The global lithium resource extraction mainly adopts salt lake lithium extraction and ore lithium extraction. For the ore lithium extraction process, it mainly includes limestone method, sulfuric acid method, sulfate method, chloride method and pressure cooking method. The above methods all use leaching and crystallization processes for concentration. For example, the methods for preparing lithium carbonate from lithium mica ore as a resource mainly include acid method, alkali method and salt method. Among them, the acid method mainly uses sulfuric acid as a leaching agent, and it is necessary to pre-defluorinate and roast at high temperature to destroy the mica structure, or add sulfuric acid to roast, and then leaching. The alkali method mainly adds calcium carbonate to roast at high temperature and then leaches, or defluorinates and roasts at high temperature and then leaches under alkaline conditions. The salt method mixes sulfate, chloride, etc. with lithium mica and then calcines at high temperature to extract lithium. The sulfate method generally uses potassium sulfate, which is expensive; the chloride method produces chlorine gas, which seriously corrodes the equipment, and the chloride ion in the lithium carbonate product is easy to exceed the standard, so there are many deficiencies or defects.

[0003] Patent CN 117210703 A discloses a method for extracting lithium from lithium-containing ores, which discloses that mixed acid treatment can overcome the above problems. For example, it discloses that: in step S1, lithium-containing ore powder is reacted with mixed acid and water to obtain an acidified slurry, and the mixed acid includes mixed acid (410 ml of 31% hydrochloric acid, 110 ml of 98% sulfuric acid, and 200 ml of 36% fluorosilicic acid) mixed, and reacted at 80°C for 10 hours to obtain an acidified slurry. The lithium-containing ore powder is acidified to dissolve its main components in the slurry in the form of ions, and the filtrate is obtained by filtering and eluting. After cooling and precipitation of alum, it is treated by membrane method to obtain a concentrated lithium-rich solution, and finally lithium is extracted by extraction process. The membrane method treatment, for example, can specifically be carried out by four-stage nanofiltration impurity removal and reverse osmosis concentration treatment on the alum precipitation mother liquor to remove multivalent impurity ions and obtain a lithium-rich solution. At the same time, the above impurity ions can be recycled: for example, if nanofiltration is used for impurity removal, the mixed solution after cooling and precipitation of alum is usually stored in the original liquid tank, and after passing through the primary pretreatment membrane, the carbonate and sulfate are separated and discharged, and the primary pretreatment membrane water produced by removing carbonate and sulfate is collected in the primary liquid tank, and the primary pretreatment liquid in the primary liquid tank is then filtered through the secondary booster to obtain the concentrated liquid and concentrated water of the secondary nanofiltration section. The anionic substances in the concentrated water mainly include fluoride ions and chloride ions. The fluoride ions in the above concentrated water can be used to prepare hydrofluoric acid, thereby providing a route for resource recovery of hydrofluoric acid, but how to carry out a good resource recovery route is not mentioned. In fact, how to recycle the above anions for reuse has always been a difficult problem in the treatment of concentrated water in this step. For example, the prior art mainly has the following routes for recycling and preparing hydrofluoric acid: the first is to absorb the acidic anions by the alkali solution method; the second is to absorb the fluoride ions by calcium ions. However, the above two methods cannot directly recover hydrofluoric acid. The salt solution or CaF after neutralization with alkali solution still needs to be treated again to obtain hydrofluoric acid. Therefore, the concentrated water in the above treatment section still has the disadvantages of complicated operation and steps in the recovery of hydrofluoric acid. Summary of the invention

[0004] To solve the problems existing in the prior art, the present invention provides a method for recovering concentrated water from lithium extraction leachate from lepidolite ore by nanofiltration membrane. This application takes concentrated water obtained from a lithium extraction method for lithium-containing ore disclosed in patent CN 117210703 A as an example, and solves the recovery problem existing in the above concentrated water treatment.

[0005] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:

[0006] A method for recovering concentrated water from a nanofiltration membrane section of a lithium leaching solution from a lepidolite mine, comprising the following steps:

[0007] 1) heating and evaporating the concentrated water collected after the nanofiltration membrane treatment to remove part of the water;

[0008] 2) adding sulfuric acid to the concentrated solution after preliminary dehydration in step 1), wherein the amount of sulfuric acid added accounts for 10-15% of the mass of the concentrated water in step 1); then heating at 110-120° C. to evaporate and remove chloride ions, and the heating time is 15-24 hours;

[0009] 3) On the basis of step 2), sulfuric acid is continued to be added, wherein the amount of sulfuric acid added is 1.5 to 1.6 times the mass of the concentrated water in step 1); then heating is performed at 150 to 160° C., and water is added during the heating process to evaporate and remove fluoride ions, and the heating time is 18 to 36 hours.

[0010] Preferably, the volume fraction of sulfuric acid used is 98%.

[0011] Preferably, the amount of deionized water added in step 3) is 25-30% of the mass of concentrated water.

[0012] The applicant has found that the concentration and amount of sulfuric acid added in steps, the heating temperature used, and the amount of water added in step 3) will greatly affect the effect of recovering chloride ions and fluoride ions. The above processes need to be properly coordinated to obtain better recovery of fluoride ions and chloride ions to directly absorb hydrogen fluoride and hydrogen chloride.

[0013] Preferably, in step 1), the concentrated water collected after the nanofiltration membrane treatment is heated at 90-100° C. until 40-60% of the water is evaporated and removed.

[0014] Preferably, the concentrated water comes from lithium extraction from lepidolite ore by a mixed acid process, wherein the mixed acid comprises hydrochloric acid, sulfuric acid and fluorosilicic acid.

[0015] Preferably, the nanofiltration membrane segment includes multiple stages of nanofiltration, and the concentrated water is collected from any nanofiltration membrane segment or the concentrated water after the multiple stages of nanofiltration are combined.

[0016] The present invention also provides a method for directly obtaining hydrogen chloride and hydrofluoric acid, which comprises the following steps:

[0017] 1) heating and evaporating concentrated water collected from lithium extraction leaching solution of lepidolite ore or its leaching solution after being treated by nanofiltration membrane section to remove part of water;

[0018] 2) adding sulfuric acid to the concentrated solution after preliminary water removal in step 1), wherein the amount of sulfuric acid added accounts for 10-15% of the mass of the concentrated water in step 1); then heating at 110-120° C. for 15-24 hours, collecting the evaporated liquid to obtain hydrogen chloride;

[0019] 3) On the basis of step 2), sulfuric acid is continued to be added, wherein the amount of sulfuric acid added is 1.5 to 1.6 times the mass of the concentrated water in step 1); then heating is performed at 150 to 160° C., water is replenished and evaporated during the heating process, the heating time is 18 to 36 hours, and the evaporated liquid is collected to obtain hydrogen fluoride.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention can directly recover hydrogen chloride and hydrofluoric acid from the concentrated water by adding sulfuric acid to the concentrated water obtained in the nanofiltration stage in multiple steps, and at the same time combining auxiliary separation at different temperatures. The method adopted by the present invention can directly evaporate the fluorine ions and chloride ions in the concentrated water section to obtain the target product (liquid), without the need for secondary extraction and purification, and the raw materials are easy to obtain and the operation is simple. Not only can the concentrated water section be simplified for recycling, but also the corresponding product can be directly obtained in one step, providing a good recycling strategy for the resource utilization of chloride ions and fluoride ions in concentrated water. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of a method for recovering concentrated water from a nanofiltration membrane section of a lithium leaching solution from a lepidolite mine provided in this application;

[0023] Figure 2 This is the result obtained by real-time detection in step 3) of Example 1. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Unless otherwise specified, the experimental methods used in the examples of the present invention are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0026] The concentrated water of the nanofiltration membrane section of the lithium leaching solution of the lepidolite ore in this embodiment can refer to the concentrated water obtained by the nanofiltration membrane section in patent CN 117210703 A. The following embodiment recovers the concentrated water. Using the above patent method, this embodiment obtains 2N concentrated water, and its composition is as follows:

[0027] Ion type <![CDATA[F - / ppm]]> <![CDATA[Cl - / ppm]]> <![CDATA[SO4 2- / ppm]]> Al / ppm Ca / ppm Fe / ppm K / ppm concentration 25724.48 53325.47 1734.89 24600.75 204.34 4711.75 425.24 Ion type Li / ppm Mg / ppm Mn / ppm Na / ppm Rb / ppm Si / ppm concentration 35.21 279.45 652.12 5.18 47.51 0

[0028] It can be seen from the above concentrated water that the concentration of fluoride ions and chloride ions present as anions is very high and needs to be recycled. This application uses the above concentrated water section for recycling. The above is also applicable to the direct recovery and extraction of lithium leaching solution from lepidolite ore, which is not limited in this application.

[0029] Example 1

[0030] like Figure 1 As shown, a method for recovering concentrated water from a nanofiltration membrane section of a lithium leaching solution from a lepidolite ore comprises the following steps:

[0031] 1) The concentrated water collected after the nanofiltration membrane treatment is heated at 95° C. until 50% of the water is evaporated;

[0032] 2) adding sulfuric acid to the concentrated solution after preliminary water removal in step 1), wherein the amount of sulfuric acid added accounts for 11% of the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then heating at 115° C. to evaporate and remove chloride ions, and the heating time is 18 hours;

[0033] 3) On the basis of step 2), sulfuric acid is continued to be added, wherein the amount of sulfuric acid added is 1.5 times the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then heating is carried out at 160°C, and water is replenished during the heating process. The amount of deionized water added is 30% of the mass of the concentrated water. This process is used to evaporate and remove fluoride ions, and the heating time is 24 hours.

[0034] Example 2

[0035] A method for recovering concentrated water from a nanofiltration membrane section of a lithium leaching solution from a lepidolite mine, comprising the following steps:

[0036] 1) The concentrated water collected after the nanofiltration membrane treatment is heated at 90° C. until 40% of the water is evaporated;

[0037] 2) adding sulfuric acid to the concentrated solution after preliminary water removal in step 1), wherein the amount of sulfuric acid added accounts for 12% of the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then heating at 110° C. to evaporate and remove chloride ions, and the heating time is 24 hours;

[0038] 3) On the basis of step 2), sulfuric acid is continued to be added, wherein the amount of sulfuric acid added is 1.6 times the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then heating is carried out at 150°C, and water is replenished during the heating process. The amount of deionized water added is 25% of the mass of the concentrated water. This process is used to evaporate and remove fluoride ions, and the heating time is 36 hours.

[0039] Example 3

[0040] A method for recovering concentrated water from a nanofiltration membrane section of a lithium leaching solution from a lepidolite mine, comprising the following steps:

[0041] 1) The concentrated water collected after the nanofiltration membrane treatment is heated at 100° C. until 60% of the water is evaporated;

[0042] 2) adding sulfuric acid to the concentrated solution after preliminary water removal in step 1), wherein the amount of sulfuric acid added accounts for 10% of the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then heating at 120° C. to evaporate and remove chloride ions, and the heating time is 15 hours;

[0043] 3) On the basis of step 2), sulfuric acid is continued to be added, wherein the amount of sulfuric acid added is 1.55 times the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then heating is carried out at 155°C, and water is replenished during the heating process. The amount of deionized water added is 28% of the mass of the concentrated water. This process is used to evaporate and remove fluoride ions, and the heating time is 18 hours.

[0044] Comparative Example 1

[0045] The other experimental steps are the same as those in Example 1, except that: Step 2) sulfuric acid is added to the concentrated solution after preliminary dehydration in Step 1), wherein the amount of sulfuric acid added accounts for 5% of the mass of the concentrated water in Step 1), and the volume fraction of sulfuric acid is 98%; then the solution is heated at 115°C to evaporate and remove chloride ions, and the heating time is 18 hours.

[0046] Comparative Example 2

[0047] The other experimental steps are the same as those in Example 1, except for step 3): sulfuric acid is continued to be added on the basis of step 2), wherein the amount of sulfuric acid added is 1 times the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then the mixture is heated at 160°C, and water is replenished during the heating process. The amount of deionized water added is 30% of the mass of the concentrated water. This process is used to evaporate and remove fluoride ions, and the heating time is 24 hours.

[0048] Comparative Example 3

[0049] The other experimental steps are the same as those in Example 1, except for step 3): sulfuric acid is continued to be added on the basis of step 2), wherein the amount of sulfuric acid added is 1.5 times the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then the mixture is heated at 120°C, and water is replenished during the heating process. The amount of deionized water added is 30% of the mass of the concentrated water. This process is used to evaporate and remove fluoride ions, and the heating time is 24 hours.

[0050] Comparative Example 4

[0051] The other experimental steps are the same as those in Example 1, except for step 3): sulfuric acid is continued to be added on the basis of step 2), wherein the amount of sulfuric acid added is 1.5 times the mass of the concentrated water in step 1), and the volume fraction of sulfuric acid is 98%; then the mixture is heated at 160°C, and water is replenished during the heating process, and the amount of deionized water added is 15% of the mass of the concentrated water. This process is used to evaporate and remove fluoride ions, and the heating time is 24 hours.

[0052] Comparative Example 5

[0053] The other experimental steps are the same as those in Example 1, except that the volume fraction of sulfuric acid used is 50%.

[0054] Effect verification: The concentrated water extraction effects of the embodiment and the comparative example were tested: the test instrument was an ion chromatograph (Shenghan CIC-D100). The analysis test conditions were: chromatographic column model: SH-AC-23 (4.0mm*m250mm); eluent: 15mM NaOH; flow rate: 1.0mL / min; injection volume: 25uL; pressure: 10.6MPa; column temperature: 35℃; detector: suppression conductance current: 50mA.

[0055] one, Figure 2 Table 1 shows the results of the instant detection in step 3) of Example 1:

[0056] Table 1

[0057] Compound Name Retention time [min] Peak area [(μS / cm)*min] Peak height [μS / cm] Separation Tailing Factor fluorine 3.30 5.55 36.63 14.21 2.08 chlorine 4.82 ND (Not Detected, the same below) ND ND ND

[0058] 2. The chloride ions and chloride ion concentrations obtained in each step were compared before and after treatment in each embodiment and comparative example, wherein ① chlorine absorption percentage = the mass of chloride ions absorbed after each step / the mass of chloride ions in the concentrated water taken in step 1) × 100%; ② fluorine absorption percentage = the mass of fluorine ions absorbed after each step / the mass of fluorine ions in the concentrated water taken in step 1) × 100%. Specific test and calculated data are shown in Table 2 below:

[0059] Table 2

[0060]

[0061] As can be seen from Table 2, after the treatment in step 2), the absorption of chloride ions in Examples 1 to 3 is good, all reaching more than 95%, that is, basically all recovery can be achieved. Although the absorption of fluorine is affected in the step 2), that is, the fluorine ions are taken out of the absorption liquid in step 2), but the amount taken out is small; the fluorine can be basically completely absorbed in the step 3), and there is no mutual influence, that is, hydrogen fluoride and hydrogen chloride solutions with good purity and extraction concentration can be directly obtained to complete the recovery.

[0062] In addition, in comparative example 1, in step 2), the amount of sulfuric acid added is 5% of the mass of the concentrated water in step 1). The amount of sulfuric acid used is small, which affects the complete absorption of chloride ions in this process, thereby causing the chloride ions and fluoride ions in the subsequent steps to still be mixed together in large quantities, and a good separation and recovery effect is not achieved. At the same time, after step 3), the fluoride ions cannot be completely extracted, affecting the recovery effect.

[0063] In comparative example 2, sulfuric acid accounting for 1 times the mass of the concentrated water in step 1) is added during the extraction process of step 3). This amount also affects the complete extraction effect of fluoride ions in step 3). The fluoride ion concentration obtained in the final treatment is 39.00%, which cannot achieve a good recovery effect.

[0064] In comparative example 3, the extraction process in step 3) is heated at 120° C. This temperature cannot achieve a good coordination effect with sulfuric acid. The fluoride ion concentration obtained in the final treatment is 28.00%, and the absorption of fluoride ions is very low.

[0065] In comparative example 4, the amount of deionized water added in step 3) is 15% of the mass of concentrated water. It can be clearly seen from Table 2 that the water added in this proportion cannot cooperate well with sulfuric acid to extract fluoride ions. The fluoride ion concentration obtained after step 3) is 58.50%, and a large amount of fluoride ions cannot be extracted.

[0066] Comparative Example 5 provides a process using sulfuric acid at a concentration of 50% by volume. It can be found that the concentration of chloride ions extracted is only 40.39%, which also affects the subsequent extraction of fluoride ions, resulting in a poor effect.

[0067] Run the experiment:

[0068] The method of the present invention is used to collect concentrated water from the nanofiltration membrane, combined with the method of Example 1 for real-time recovery, and industrial continuous recovery treatment is carried out. Various process indicators are stable, and hydrogen fluoride and hydrogen chloride can be directly recovered, which has good industrial recovery value.

[0069] The specific implementation scheme described above is only a further detailed description of the purpose, technical scheme and beneficial effects of the present invention. It should be understood that the above is only a specific example of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for recovering concentrated water from a lithium leaching solution from a lepidolite mine by using a nanofiltration membrane, characterized in that: The steps include: 1) heating and evaporating the concentrated water collected after the nanofiltration membrane treatment to remove part of the water; 2) adding sulfuric acid to the concentrated solution after preliminary dehydration in step 1), wherein the amount of sulfuric acid added accounts for 10-15% of the mass of the concentrated water in step 1); then heating at 110-120° C. for 15-24 hours to evaporate and remove chloride ions; 3) On the basis of step 2), sulfuric acid is continued to be added, wherein the amount of sulfuric acid added is 1.5 to 1.6 times the mass of the concentrated water in step 1); then heating is performed at 150 to 160° C. for 18 to 36 hours to evaporate and remove fluoride ions.

2. The method for recovering concentrated water from lithium leaching solution from lepidolite ore by nanofiltration membrane section according to claim 1, characterized in that: In step 3), water is replenished during the heating process.

3. The method for recovering concentrated water from lithium leaching solution from lepidolite ore by nanofiltration membrane section according to claim 2, characterized in that: In step 3), water is added during the heating process to evaporate and remove fluoride ions, and the amount of added water is 25-30% of the mass of the concentrated water in step 1).

4. The method for recovering concentrated water from lithium leaching solution from lepidolite ore by nanofiltration membrane section according to claim 1, characterized in that: The volume fraction of sulfuric acid used is 70-98%.

5. The method for recovering concentrated water from lithium leaching solution of lepidolite ore by nanofiltration membrane section according to claim 1, characterized in that: In step 1), the concentrated water collected after the nanofiltration membrane treatment is heated at 90-100° C. until 40-60% of the water is evaporated and removed.

6. The method for recovering concentrated water from lithium leaching solution from lepidolite ore by nanofiltration membrane section according to claim 1, characterized in that: The concentrated water comes from the mixed acid method of lithium extraction from lepidolite ore, and the mixed acid includes hydrochloric acid, sulfuric acid and fluorosilicic acid.

7. The method for recovering concentrated water from lithium leaching solution from lepidolite ore by nanofiltration membrane section according to claim 6, characterized in that: The nanofiltration membrane section includes multiple stages of nanofiltration, and concentrated water is collected from any nanofiltration membrane section or the concentrated water after the multiple stages of nanofiltration are combined.

8. A method for directly obtaining hydrogen chloride and hydrofluoric acid, characterized in that: The method is to extract the lithium from a lithium mica ore using a lithium leaching solution, or to recover the concentrated water from the lithium leaching solution of a lithium mica ore after filtering it through a nanofiltration membrane section, comprising the following steps: 1) heating and evaporating concentrated water collected from lithium extraction leaching solution of lepidolite ore or its leaching solution after being treated by nanofiltration membrane section to remove part of water; 2) adding sulfuric acid to the concentrated solution after preliminary water removal in step 1), wherein the amount of sulfuric acid added accounts for 10-15% of the mass of the concentrated water in step 1); then heating at 110-120° C. for 15-24 hours, collecting the evaporated liquid to obtain hydrogen chloride; 3) adding sulfuric acid based on step 2), wherein the amount of sulfuric acid added is 1.5 to 1.6 times the mass of the concentrated water in step 1); Then, the mixture is heated at 150-160° C., water is added and evaporated during the heating process, and the heating time is 18-36 hours. The evaporated liquid is collected to obtain hydrogen fluoride.

9. A method for directly obtaining hydrogen chloride and hydrofluoric acid according to claim 8, characterized in that: The liquid collected from hydrogen chloride and hydrogen fluoride in step 2) and step 3) is water.

Citation Information

Patent Citations

  • Lithium extraction method for lithium-containing ore

    CN117210703A

  • Method for recycling sulfuric acid and hydrochloric acid from smelting wastewater and realizing fluorine open circuit

    CN105461138A

  • Treatment method for removing fluorine and chlorine ions in acidic wastewater

    CN105731704A

  • Recovery apparatus of fluorine aqueous solution or hydrofluoric acid aqueous solution, its recovery method, and circulating and using system of the same

    JP2004091224A

  • Method for recovering mixed acid with increased hydrochloric acid concentration from hydrochloric acid-hydrofluoric acid-based mixed acid waste liquid

    JP2011001246A