Binder and preparation method thereof, and molding process of hollow glass beads sprayed by binder

By using specific formula binders and spray printing technology to mold hollow glass microbeads, combined with thermal isostatic sintering and sandblasting treatment, the problem of difficult to form complex structures in the existing technology is solved, and efficient and rapid finished product production is achieved .

CN118978331APending Publication Date: 2024-11-19BEIJING SANDI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049150.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to form hollow glass microbeads with complex lattice structures, which limits their application in special purposes.

Method used

Using a binder, including silicone resin, isopropanol, ethylene glycol, glacial acetic acid, alcohol, phenolic resin, furfuryl alcohol and silane coupling agent, hollow glass microbeads are formed by jet printing technology and cured in an oven. Afterwards, thermal isostatic sintering and sandblasting are carried out.

Benefits of technology

The formation of hollow, complex and dot matrix structures is achieved, with the ultimate wall thickness and aperture reaching 1mm, the forming speed is fast, the production cycle is reduced, and the degree of automation and yield is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a binder, a preparation method of the binder and a molding process of hollow glass beads sprayed by the binder, and belongs to the technical field of binder spray molding. Wherein the binder comprises organic silicon resin, isopropanol, ethylene glycol, glacial acetic acid, alcohol powder, phenolic resin, furfuryl alcohol, a silane coupling agent and ethylene glycol butyl ether. The forming process comprises the following steps: screening the hollow glass beads; putting the glass beads and the binder into corresponding positions of a binder jet printer, slicing according to a required model, and importing a slicing file into equipment for forming; after forming is completed, the forming cylinder is put into a drying oven to be baked, and a glass piece is obtained after curing; and taking out the glass piece, and carrying out cleaning, degreasing, hot isostatic pressing sintering and sand blasting treatment to obtain a finished product. The forming process is high in forming speed, and the manufacturing period is shortened; the automation degree is high, and the yield is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of binder spraying molding, and more particularly to a binder and a preparation method thereof, and a binder spraying hollow glass microbead molding process. Background Art

[0002] With the development of science and technology, hollow glass microspheres have been industrialized, making them a new type of inorganic material with low price and abundant resources. They have excellent performance. With good product performance and relatively low market price, they have been widely used in military and civilian fields such as thermal insulation and fireproof materials, advanced insulation materials, composite materials, petrochemicals, and coatings.

[0003] The use of binder jetting technology to form hollow glass microspheres can achieve higher optical quality, design flexibility and strength. It can produce hollow, complex, and lattice structures with excellent performance and is more suitable for special uses in aviation, petroleum, and military. Summary of the Invention

[0004] In view of this, the present invention provides a binder, a preparation method thereof, and a binder-injected hollow glass microsphere molding process. The present invention can be used to mold hollow glass microspheres with complex structures, expanding the variety of uses for hollow glass microspheres and enabling applications that are not possible with traditional craft products.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A binder comprises the following components in parts by weight: 75-100 parts of silicone resin, 25-50 parts of isopropyl alcohol, 5-10 parts of ethylene glycol, 5-10 parts of glacial acetic acid, 100-200 parts of alcohol, 75-100 parts of phenolic resin, 150-200 parts of furfuryl alcohol, 20-40 parts of silane coupling agent, and 4-6 parts of ethylene glycol butyl ether.

[0007] Another object of the present invention is to provide a method for preparing the above-mentioned binder, comprising the following steps:

[0008] (1) Weigh each component of the above-mentioned binder and set aside;

[0009] (2) Stirring the alcohol and phenolic resin under heating conditions for 1 hour to obtain a mixed solution, which is set aside;

[0010] (3) The silicone resin and isopropyl alcohol were stirred and mixed under heating conditions for 10 minutes, and then ethylene glycol and glacial acetic acid were added and stirred and mixed for 30 minutes, and then furfuryl alcohol and ethylene glycol butyl ether were added and stirred and mixed for 1 hour to obtain a mixed solution II;

[0011] (4) Mixing the second mixed solution with the first mixed solution, cooling the mixture, then adding a silane coupling agent, and continuing to stir and mix for 30 minutes to obtain the adhesive.

[0012] Preferably, the heating in step (2) is heating to 50° C.; and the stirring and mixing speed is 350 rpm / min.

[0013] Preferably, the heating in step (3) is heating to 90° C., and the stirring and mixing speed is 260 rpm / min.

[0014] Preferably, the cooling in step (4) is to 70° C., and the stirring and mixing speed is 260 rpm / min.

[0015] Another object of the present invention is to provide a binder-injected hollow glass microsphere molding process, comprising the following steps:

[0016] S1, sieving the hollow glass microspheres to control the particle size to 70-140 mesh;

[0017] S2, placing glass beads and the above-mentioned binder in the corresponding position of the binder jet printer, slicing according to the required model, and importing the slice file into the device for molding;

[0018] S3, after the molding is completed, the molding cylinder is placed in an oven for baking, and the glass piece is obtained after solidification;

[0019] S4, after the glass pieces are taken out, they are cleaned, degreased, hot isostatically pressed and sandblasted to obtain the finished product.

[0020] Preferably, the baking temperature in step S3 is 180-200° C. and the baking time is 2 hours.

[0021] Preferably, the sintering pressure of the hot isostatic pressing sintering is 10-20 MPa.

[0022] It can be seen from the above technical solutions that compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) Structural limitations can be ignored, and hollow, complex, and lattice structures that cannot be achieved with traditional technologies can be formed;

[0024] (2) The maximum wall thickness and hole diameter can reach 1mm, which can process various fine workpieces;

[0025] (3) The molding speed is fast, which reduces the production cycle; the degree of automation is high, which improves the yield rate. DETAILED DESCRIPTION

[0026] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0027] Example 1

[0028] This embodiment provides an adhesive, which includes the following components by weight:

[0029] 75 parts of silicone resin, 25 parts of isopropyl alcohol, 7 parts of ethylene glycol, 5 parts of glacial acetic acid, 120 parts of alcohol, 75 parts of phenolic resin, 150 parts of furfuryl alcohol, 20 parts of silane coupling agent, and 4 parts of ethylene glycol butyl ether.

[0030] The preparation method is:

[0031] (1) Weigh each component of the above-mentioned binder and set aside;

[0032] (2) Mix the alcohol and phenolic resin, heat to 50°C, and stir at 350 rpm / min for 1 hour to obtain a mixed solution 1, which is set aside;

[0033] (3) The silicone resin and isopropyl alcohol were mixed, heated to 90° C., and stirred at 260 rpm / min for 10 min. Ethylene glycol and glacial acetic acid were then added, and stirred at 260 rpm / min for 30 min. Furfuryl alcohol and ethylene glycol butyl ether were then added, and stirred at 260 rpm / min for 1 h to obtain a second mixed solution.

[0034] (4) Mix the mixed solution 2 and the mixed solution 1, cool the mixture to 70° C., then add a silane coupling agent, and stir and mix at a speed of 260 rpm / min for 30 minutes to obtain a binder.

[0035] Example 2

[0036] This embodiment provides an adhesive, which includes the following components by weight:

[0037] 90 parts of silicone resin, 40 parts of isopropyl alcohol, 8 parts of ethylene glycol, 6 parts of glacial acetic acid, 150 parts of alcohol, 90 parts of phenolic resin, 180 parts of furfuryl alcohol, 25 parts of silane coupling agent, and 5 parts of ethylene glycol butyl ether.

[0038] The preparation method is the same as that of Example 1.

[0039] Example 3

[0040] This embodiment provides an adhesive, which includes the following components by weight: 100 parts of silicone resin, 50 parts of isopropyl alcohol, 9 parts of ethylene glycol, 9 parts of glacial acetic acid, 180 parts of alcohol, 90 parts of phenolic resin, 160 parts of furfuryl alcohol, 35 parts of silane coupling agent, and 6 parts of ethylene glycol butyl ether.

[0041] The preparation method is the same as that of Example 1.

[0042] Example 4

[0043] This embodiment provides a binder-injected hollow glass microsphere molding process, comprising the following steps:

[0044] (1) First, design a 3D model of the glass part, cut it into a CLI format file using slicing software, and import it into the binder jet printer;

[0045] (2) Screening the hollow glass microspheres to control the particle size to 70 mesh;

[0046] (3) Place the hollow glass microspheres and the binder in the corresponding positions of the binder jet printer;

[0047] (4) Slice the file in CLI format and print the glass 3D model;

[0048] (5) After printing is completed, the molding cylinder is placed in an oven at 180°C for 2 hours to complete the curing;

[0049] (6) The glass parts are taken out and cleaned to remove the floating powder. The glass parts are placed in a degreasing furnace for degreasing. The glass parts are then placed in a hot isostatic pressing furnace for hot isostatic pressing at a pressure of 20 MPa. The glass parts are then sandblasted to form the final product.

[0050] Example 5

[0051] This embodiment provides a binder-injected hollow glass microsphere molding process, comprising the following steps:

[0052] (1) First, design a 3D model of the glass part, cut it into a CLI format file using slicing software, and import it into the binder jet printer;

[0053] (2) Screening the hollow glass microspheres to control the particle size to 140 mesh;

[0054] (3) Place the hollow glass microspheres and the binder in the corresponding positions of the binder jet printer;

[0055] (4) Slice the file in CLI format and print the glass 3D model;

[0056] (5) After printing is completed, the molding cylinder is placed in an oven at 200°C for 2 hours to complete the curing;

[0057] (6) The glass parts are taken out and cleaned to remove the floating powder. The glass parts are placed in a degreasing furnace for degreasing. The glass parts are then placed in a hot isostatic pressing furnace for hot isostatic pressing at a pressure of 10 MPa. The glass parts are then sandblasted to form the final product.

[0058] The molding process of the present invention is compared with the prior art, and the results are shown in Table 1 below:

[0059] Table 1

[0060] Processing method Molding method Molding speed Production cycle Binder Jetting Direct molding + debinding sintering <![CDATA[3000-5000cm 3 / h]]> 2-3 days Laser sintering Direct molding + debinding sintering <![CDATA[90-150cm 3 / h]]> 5-7 days Traditional crafts Mold + hot pressing / 15-20 days

[0061] As can be seen from the above table, the binder-jet hollow glass microsphere molding process provided by the present invention has a fast molding speed, shortens the production cycle, has a high degree of automation, and improves the yield rate.

[0062] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. Reference can be made to the common and similar parts between the various embodiments. For the devices disclosed in the embodiments, since they correspond to the methods disclosed in the embodiments, the description is relatively simple, and the relevant parts can be referred to the method description.

[0063] The above description of the disclosed embodiments is intended to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be readily apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not limited to the embodiments shown herein but is intended to conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A binder, characterized in that: The composition includes the following ingredients in parts by weight: 75-100 parts of silicone resin, 25-50 parts of isopropyl alcohol, 5-10 parts of ethylene glycol, 5-10 parts of glacial acetic acid, 100-200 parts of alcohol, 75-100 parts of phenolic resin, 150-200 parts of furfuryl alcohol, 20-40 parts of silane coupling agent and 4-6 parts of ethylene glycol butyl ether.

2. A method for preparing a binder, characterized in that: The following steps are involved: (1) Weighing each component of the binder according to claim 1 and setting aside; (2) stirring and mixing the alcohol and phenolic resin under heating conditions for 1 h to obtain a mixed solution 1 for standby use; (3) stirring and mixing the silicone resin and isopropanol under heating conditions for 10 minutes, then adding ethylene glycol and glacial acetic acid and stirring and mixing for 30 minutes, and then adding furfuryl alcohol and ethylene glycol butyl ether and stirring and mixing for 1 hour to obtain a mixed solution II; (4) Mixing the mixed solution 2 with the mixed solution 1, cooling the mixture, adding a silane coupling agent, and continuing to stir and mix for 30 minutes to obtain the adhesive.

3. A binder spraying hollow glass microsphere forming process according to claim 2, characterized in that: The heating in step (2) is heating to 50° C.; the stirring and mixing speed is 350 rpm / min.

4. The binder-injection hollow glass microsphere forming process according to claim 2, characterized in that: The heating in step (3) is to heat to 90° C., and the stirring and mixing speed is 260 rpm / min.

5. The binder-injection hollow glass microsphere forming process according to claim 2, characterized in that: The cooling in step (4) is to cool to 70° C., and the stirring and mixing speed is 260 rpm / min.

6. A binder-injected hollow glass microsphere forming process, characterized in that: The following steps are involved: S1, sieving the hollow glass microspheres to control the particle size to 70-140 mesh; S2, placing the glass beads and the binder according to claim 1 into corresponding positions of the binder jet printer, slicing according to the required model, and importing the slice file into the device for molding; S3, after the molding is completed, the molding cylinder is placed in an oven for baking, and the glass piece is obtained after solidification; S4, after the glass parts are taken out, they are cleaned, degreased, hot isostatically pressed and sintered, and sandblasted to obtain the finished product.

7. The binder-injection hollow glass microsphere forming process according to claim 6, characterized in that: The baking temperature in step S3 is 180-200° C. and the baking time is 2 hours.