Method for preparing refractory material from ardealite flotation black carbon-silicon tailings
By heating the black carbon-silicon tailings of phosphogypsum flotation with coal gasification slag at high temperature and mixing them with magnesium-aluminum spinel, composite refractory materials are prepared, which solves the problems of tailings accumulation and environmental pollution, and achieves efficient utilization of resources and Low energy consumption and high strength properties of refractory materials.
Patent Information
- Application Number
- CN202411032896.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The amount of black carbon silicon tailings produced during the preparation process of phosphogypsum wet phosphate dihydrate method is large, which leads to environmental pollution. It is necessary to find effective ways of utilization.
Silicon carbide or silicon carbon nitride powder is prepared by heating the black carbon gypsum flotation with the gasification slag at high temperature, mixing it with magnesium-aluminum spinel, and using pickling and impurity removal and high-temperature reactions, and is used to prepare silicon carbide or silicon carbon nitride powder, and is combined with aluminum ash Combining acid slag dissolving, alumina powder, metal aluminum powder and other materials, they are formed by hydraulic presses or friction brick presses to prepare composite refractory materials.
The accumulation of black carbon silicon tailings is significantly reduced, and the efficient utilization of resources is achieved. The prepared refractory materials have good mechanical strength in the medium and low temperature and high temperature stages, and have low energy consumption.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature refractory materials, and in particular to a method for utilizing black carbon silicon tailings from phosphogypsum flotation. Background Art
[0002] In the process of preparing phosphogypsum by the phosphorus chemical industry's wet phosphoric acid dihydrate method, a large amount of black carbon silicon tailings are produced under the action of enhanced flotation. Its main component is silicon, and its main form is silicon dioxide. After centralized collection, it was found that its output was too large. About 100kg of black carbon silicon tailings will be produced for every ton of high-purity phosphogypsum. The large output and excessive accumulation are likely to cause environmental pollution, and it is urgent to find a way to utilize it.
[0003] Silicon carbide is an important non-oxide refractory material used in high-temperature kilns due to its excellent high-temperature wear resistance, erosion resistance, thermal shock resistance and high thermal conductivity.
[0004] CN202210830247.0 provides a method for preparing a fire-free silicon carbide-magnesium aluminum spinel refractory material, that is, adding alumina powder and metal aluminum powder to silicon carbide material and magnesium aluminum spinel powder, and adding aluminum dihydrogen phosphate powder and liquid organic resin, and the raw materials and binders are mixed evenly and then formed on a hydraulic press or a friction brick press at 110-150MPa pressure, and then placed at room temperature for 12-18 hours and dried at 180-200°C for 18-24 hours to obtain the fire-free refractory material. The mechanical strength of the fire-free refractory material in the medium-low temperature and high temperature stages can be guaranteed. Summary of the invention
[0005] The object of the present invention is to provide a method for treating phosphogypsum flotation tailings, which can significantly reduce the accumulation of phosphogypsum flotation tailings, reduce environmental pollution, and optimize resource utilization.
[0006] In order to achieve the purpose of resource utilization of this black carbon silicon slag, the present invention adopts the following technical scheme: The present invention provides a method for utilizing phosphogypsum flotation tailings, wherein black carbon silicon tailings of phosphogypsum flotation are heated at high temperature in coordination with coal gasification slag, and then mixed with magnesium aluminum spinel to prepare a composite refractory material, the method comprising the following steps: (1) Wash the black carbon silicon tailings from the flotation of phosphogypsum with water at a temperature of 80-100°C, which is 2-3 times the weight of the tailings to be washed, to wash away the soluble phosphorus and fluorine in the black carbon silicon tailings; (2) After washing, the black carbon silicon tailings are dried in an oven at 80-100°C for 5-10h, the dried tailings are mixed with coal gasification slag, coke is added, and the black carbon silicon tailings and coal gasification slag are pickled with a 5-20wt% sulfuric acid solution at a temperature of 60-80°C to remove metal oxide impurities such as Al2O3 and Fe2O3, and then placed in an electric furnace, heated to 1800-2200°C, and reacted for 5-10h to obtain silicon carbide powder; In some embodiments, a nitrogen source may be added before heating to finally obtain silicon carbonitride powder. The specific steps are as follows: After washing, the black carbon silicon tailings are dried in an oven at 80-100°C for 5-10h, the dried tailings are mixed with coal gasification slag, coke is added, and pickled with a 5-20wt% sulfuric acid solution at a temperature of 60-80°C to remove metal oxide impurities such as Al2O3 and Fe2O3 in the black carbon silicon tailings and coal gasification slag, and then placed in an electric furnace, a nitrogen source is added, heated to 1800-2200°C, and reacted for 5-10h to obtain silicon carbonitride powder.
[0007] The nitrogen source is selected from one or more of urea, ammonium chloride, ammonium sulfate, and ammonium nitrate. The addition amount of one or more of urea, ammonium chloride, ammonium sulfate, and ammonium nitrate is 5-10% of the mixed mass of black carbon silicon tailings from phosphogypsum flotation and coal gasification slag.
[0008] (3) The high-purity silicon carbide powder after impurity removal in step (2) is used as raw materials for refractory materials, and 3-4wt% of the weight of the raw materials are added with super polyphosphate sodium and urea-formaldehyde resin respectively. The above raw materials are mixed with a binder and then molded on a hydraulic press or a friction brick press at 130-150MPa. After being placed at room temperature for 18-20h, the mixture is dried at 180-200°C for 18-24h to obtain a silicon carbide-magnesia alumina spinel composite refractory material.
[0009] The present invention provides a method for preparing a refractory material from black carbon silicon tailings and gasification slag. The silicon in the black carbon silicon slag mainly exists in the form of active silicon dioxide, and the carbon in the coal gasification slag mainly exists in the form of active porous carbon components. Silicon carbide material can be generated through high-temperature carbonization, while other impurities are directionally enriched. Then, through the crushing and alkali washing processes at the back end, the impurities can be efficiently removed, thereby obtaining a high-purity silicon carbide material (or silicon carbonitride); the magnesia-alumina spinel obtained by desiliconization of silicon carbide and secondary aluminum ash acidolysis slag is used to prepare a refractory material under a non-burning condition. The refractory material has good mechanical strength in medium-low temperature and high temperature stages and has the advantages of low energy consumption. The refractory material is prepared by using coal gasification slag, aluminum ash acidolysis desiliconization slag and phosphogypsum flotation black carbon silicon tailings, thereby realizing the coordinated utilization of multiple solid waste resources.
[0010] According to the present invention, the SiO2 content in the black carbon silicon tailings from the flotation of phosphogypsum in step (1) is 50-80wt%, for example, it can be 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt% or 80wt%, as well as specific point values between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.
[0011] According to the present invention, the P2O5 content in the black carbon silicon tailings from the phosphogypsum flotation in step (1) is 3-10wt%, for example, 3wt%, 5wt%, 7wt%, 9wt% or 10wt%, as well as specific point values between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.
[0012] According to the present invention, the F content in the black carbon silicon tailings from the flotation of phosphogypsum in step (1) is 1-2wt%, for example, it can be 1wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt% or 2wt%, as well as specific values between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.
[0013] According to the present invention, the C content in the coal gasification slag in step (2) is 5-20wt%, for example, it can be 5wt%, 7wt%, 9wt%, 11wt%, 13wt%, 15wt%, 17wt%, 19wt% or 20wt%, as well as specific values between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.
[0014] According to the present invention, the SiO2 content in the coal gasification slag in step (2) is 40-60wt%, for example, it can be 40wt%, 42wt%, 44wt%, 46wt%, 48wt%, 50wt%, 52wt%, 54wt%, 56wt%, 58wt% or 60wt%, as well as specific values between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.
[0015] According to the present invention, the Al2O3 content in the coal gasification slag in step (2) is 10-20wt%, for example, it can be 10wt%, 12wt%, 14wt%, 16wt%, 18wt% or 20wt%, as well as specific values between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.
[0016] According to the present invention, the mass ratio of the black carbon silicon tailings from the flotation of phosphogypsum to the coal gasification slag in step (2) is (0.5-1.5):1, for example, it can be 0.5:1, 0.7:1, 0.9:1, 1.1:1, 1.3:1 or 1.5:1, as well as specific values between the above values. Due to space limitations and for the sake of simplicity, the present invention does not list them all.
[0017] According to the present invention, the mass of coke added in step (2) is 20-40wt% of the mixed mass of phosphogypsum flotation black carbon silicon tailings and coal gasification slag, for example, it can be 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 32wt%, 34wt%, 36wt%, 38wt% or 40wt% of the mixed mass of phosphogypsum flotation black carbon silicon tailings and coal gasification slag, as well as specific point values between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.
[0018] As a preferred series scheme, the method of preparing a composite refractory material by combining the black carbon silicon tailings from the flotation of phosphogypsum with the coal gasification slag and then mixing with the magnesium aluminum spinel is as follows: (1) Using water with a temperature of 80-100°C and a mass of 2-3 times the mass of the black carbon silicon tailings from phosphogypsum flotation to wash the black carbon silicon tailings; wherein the content of SiO2 in the black carbon silicon tailings from phosphogypsum flotation is 50-80wt%, the content of Al2O3 is 2-3wt%, the content of Fe2O3 is 2-3wt%, the content of F is 1-2wt%, the content of MgO is 0.2-0.5wt%, and the content of P2O5 is 3-10wt%; (2) The washed black carbon silicon tailings are dried in an oven at 80-100°C for 8-10h, mixed with coal gasification slag after drying, and then coke is added, and then pickled and impurized with a 5-20wt% sulfuric acid solution at a temperature of 60-80°C, and then placed in an electric furnace after impurities are removed, and the electric furnace is heated at 1800-2200°C and reacted for 5-10h to obtain silicon carbide raw materials; wherein the C content in the coal gasification slag is 5-20wt%, the SiO2 content is 40-60wt%, and the Al2O3 content is 10-20wt%; the mass ratio of the black carbon silicon tailings to the coal gasification slag is 0.5-1.5; the mass of the added coke is 20-40wt% of the mass of the mixture of the black carbon silicon tailings and the coal gasification slag; Alternatively, step (2) may also be: the washed black carbon silicon tailings are dried in an oven at 80-100°C for 8-10h, mixed with coal gasification slag after drying, and then coke is added, and then pickled and impurized with a 5-20wt% sulfuric acid solution at a temperature of 60-80°C, and then placed in an electric furnace after impurity removal, and a nitrogen source is added, and the electric furnace is heated to 1800-2200°C, and reacted for 5-10h to obtain silicon carbide raw materials; wherein the carbon content in the coal gasification slag is 5-20wt%, the SiO2 content is 40-60wt%, and the Al2O3 content is 10-20wt%; the mass ratio of the black carbon silicon tailings to the coal gasification slag is 0.5-1.5; the mass of the added coke is 20-40wt% of the mass of the mixture of the black carbon silicon tailings and the coal gasification slag; The nitrogen source is selected from one or more of urea, ammonium chloride, ammonium sulfate, and ammonium nitrate. The addition amount of one or more of urea, ammonium chloride, ammonium sulfate, and ammonium nitrate is 5-10% of the mixed mass of black carbon silicon tailings from phosphogypsum flotation and coal gasification slag.
[0019] (3) The high-purity silicon carbide powder after impurities removal in the above step is mixed with the magnesium-aluminum spinel prepared from the secondary aluminum ash acid decomposition slag, and alumina powder and metal aluminum powder are added, and sodium polyphosphate and urea-formaldehyde resin are added as binders. After mixing, it is pressed into shape by a hydraulic press or a friction brick press at a pressure of 130-150MPa, and then dried in an oven at 150-200℃ for 18-24h to obtain a silicon carbide-magnesium-aluminum spinel composite refractory material. Material; wherein the silicon carbide-magnesium aluminum spinel mixed raw material, the content of 0.1-3mm silicon carbide powder is 50-70wt%, the content of 20-90μm magnesium aluminum spinel fine powder is 20-30wt%, the content of D50=5-10μm alumina micropowder is 2-8wt%, and the content of 35-75μm metal aluminum powder is 2-8wt%; the addition amount of super polyphosphate sodium and urea-formaldehyde resin is 3-4wt% of the mass of the silicon carbide-magnesium aluminum spinel mixed raw material.
[0020] The invention provides a method for preparing a refractory material without firing, which can save energy consumption in large-scale industrial production and ensure the mechanical strength of the refractory material without firing at medium and low temperatures and high temperatures.
[0021] The present invention provides a utilization method of black carbon silicon tailings from phosphogypsum flotation, which can better solve the problem of large amounts of black carbon silicon tailings accumulated from phosphogypsum flotation and achieve the purpose of resource utilization. DETAILED DESCRIPTION
[0022] Example 1 This embodiment provides a method for preparing a refractory material by flotation of black carbon silicon tailings from phosphogypsum, the method comprising the following steps: (1) The black carbon silicon tailings from the flotation of phosphogypsum are washed with water at a temperature of 80°C, which is three times the weight of the washed tailings. The components and contents of the black carbon silicon tailings after washing and drying are as follows: SiO2 content is 60.8wt%, F content is 1.8wt%, and P2O5 content is 8.3wt%. The black carbon silicon tailings are mixed with coal gasification slag in a mass ratio of 0.5:1, and 40wt% of the mass of the mixture is added with coke; under heating conditions of 80°C, the mixture is washed with a 10wt% sulfuric acid solution to remove metal oxide impurities in the mixture, and the mixture is placed in an electric furnace and heated to 1800°C for 8 hours to obtain silicon carbide raw materials; (2) The high-purity silicon carbide raw material obtained in (1) above is mixed with aluminum ash acid decomposition slag and other raw materials in the following proportions: 0.1~3mm silicon carbide powder 60wt% 20~90μm magnesium aluminum spinel 30wt% D50=5~10μm alumina powder 5wt% 35~75μm aluminum powder 5wt% After mixing, 4 wt% of super sodium polyphosphate and urea-formaldehyde resin (the mass ratio of super sodium polyphosphate to urea-formaldehyde resin is 4:1) based on the raw material mass are added as bonding agents, and the mixture is molded at 150 MPa pressure on a hydraulic press or a friction brick press. After being placed at room temperature for 18 hours, the mixture is dried at 200°C for 24 hours to obtain a silicon carbide-magnesium aluminum spinel refractory material.
[0023] Example 2 This embodiment provides a method for preparing a refractory material by flotation of black carbon silicon tailings from phosphogypsum, the method comprising the following steps: (1) Wash the black carbon silicon tailings from the flotation of phosphogypsum with water at a temperature of 80°C, which is three times the weight of the washed tailings. The components and contents of the black carbon silicon tailings after washing and drying are as follows: SiO2 content is 55.7wt%, F content is 1.5wt%, and P2O5 content is 10.8wt%. The black carbon silicon tailings after washing and drying are mixed with coal gasification slag in a mass ratio of 1:1, and 30wt% of the mass of the mixture is added with coke; under heating conditions of 80°C, the mixture is washed with a 10wt% sulfuric acid solution to remove metal oxide impurities in the mixture, and the mixture is placed in an electric furnace and heated to 2000°C for 5 hours to obtain silicon carbide raw materials; (2) The high-purity silicon carbide raw material obtained in (1) above is mixed with aluminum ash acid decomposition slag and other raw materials in the following proportions: 0.1~3mm silicon carbide powder 70wt% 20~90μm magnesium aluminum spinel 20wt% D50=5~10μm alumina powder 2wt% 35~75μm aluminum powder 8wt% After mixing, 4 wt% of aluminum dihydrogen phosphate powder and urea-formaldehyde resin (the mass ratio of aluminum dihydrogen phosphate powder to urea-formaldehyde resin is 4:1) based on the raw material mass are added as bonding agents, and the mixture is molded at 150 MPa pressure on a hydraulic press or a friction brick press. After being placed at room temperature for 20 hours, the mixture is dried at 180°C for 18 hours to obtain a silicon carbide-magnesium aluminum spinel refractory material.
[0024] Example 3 This embodiment provides a method for preparing a refractory material by flotation of black carbon silicon tailings from phosphogypsum, the method comprising the following steps: (1) The components and contents of black carbon silicon tailings are as follows: SiO2 content is 50wt%, F content is 1.8wt%, P2O5 content is 9wt%, the black carbon silicon tailings after washing and drying are mixed with coal gasification slag in a mass ratio of 0.5:1, and 40wt% of the mass of the mixture is added with coke; under heating conditions of 80°C, the mixture is washed with a 10wt% sulfuric acid solution to remove metal oxide impurities in the mixture, and then placed in an electric furnace and heated to 2000°C for 5 hours to obtain silicon carbide raw material; (2) The high-purity silicon carbide raw material obtained in (1) above is mixed with aluminum ash acid decomposition slag and other raw materials in the following proportions: 0.1~3mm silicon carbide powder 65wt% 20~90μm magnesium aluminum spinel 20wt% D50=5~10μm alumina powder 8wt% 35~75μm aluminum powder 7wt% After mixing, 4 wt% of super sodium polyphosphate and urea-formaldehyde resin (the mass ratio of super sodium polyphosphate to urea-formaldehyde resin is 4:1) based on the raw material mass are added as bonding agents, and the mixture is molded at 150 MPa pressure on a hydraulic press or a friction brick press. After being placed at room temperature for 20 hours, the mixture is dried at 200°C for 24 hours to obtain a silicon carbide-magnesium aluminum spinel refractory material.
[0025] Example 4 This embodiment provides a method for preparing a refractory material by flotation of black carbon silicon tailings from phosphogypsum, the method comprising the following steps: (1) The components and contents of black carbon silicon tailings are as follows: SiO2 content is 80wt%, F content is 1wt%, P2O5 content is 3wt%, the black carbon silicon tailings after washing and drying are mixed with coal gasification slag in a mass ratio of 1.5:1, and 20wt% of the mass of the mixture is added with coke; under heating conditions of 80°C, the mixture is washed with a 10wt% sulfuric acid solution to remove metal oxide impurities in the mixture, 5wt% of urea is added, and the mixture is placed in an electric furnace and heated to 2200°C for 10 hours to obtain silicon carbonitride raw material; (2) The high-purity silicon carbonitride raw material obtained in (1) above is mixed with aluminum ash acid decomposition slag and other raw materials in the following proportions: 0.1~3mm silicon carbide powder 55wt% 20~90μm magnesium aluminum spinel 30wt% D50=5~10μm alumina powder 6wt% 35~75μm aluminum powder 9wt% After mixing, 4 wt% of super sodium polyphosphate and urea-formaldehyde resin (the mass ratio of super sodium polyphosphate to urea-formaldehyde resin is 4:1) based on the raw material mass are added as bonding agents, and the mixture is molded at 150 MPa pressure on a hydraulic press or a friction brick press. After being placed at room temperature for 18 hours, the mixture is dried at 200°C for 24 hours to obtain a silicon carbide-magnesium aluminum spinel refractory material.
[0026] Example 5 This embodiment provides a method for preparing a refractory material by flotation of black carbon silicon tailings from phosphogypsum, the method comprising the following steps: (1) The components and contents of black carbon silicon tailings are as follows: SiO2 content is 70wt%, F content is 2wt%, P2O5 content is 8wt%, the black carbon silicon tailings after washing and drying are mixed with gasification slag in a mass ratio of 1:1, and 40wt% of the mass of the mixture is added with coke; under heating conditions of 80°C, the mixture is washed with a 10wt% sulfuric acid solution to remove metal oxide impurities in the mixture, 5wt% of ammonium nitrate is added, and the mixture is placed in an electric furnace and heated to 2000°C for 5h to obtain silicon carbonitride raw material; (2) The high-purity silicon carbonitride raw material obtained in (1) above is mixed with aluminum ash acid decomposition slag and other raw materials in the following proportions: 0.1~3mm silicon carbide powder 65wt% 20~90μm magnesium aluminum spinel 30wt% D50=5~10μm alumina powder 3wt% 35~75μm aluminum powder 2wt% After mixing, 4 wt% of super polyphosphate sodium and urea-formaldehyde resin (mass ratio is 8:1) based on the raw material mass are added as bonding agents, and the mixture is molded at 150 MPa pressure on a hydraulic press or a friction brick press. After being placed at room temperature for 18 hours, the mixture is dried at 200°C for 24 hours to obtain a silicon carbide-magnesium aluminum spinel refractory material.
[0027] The characterization results of the above examples are listed in Table 1. The silicon carbide-magnesium aluminum spinel composite refractory material was subjected to a flexural test analysis at 800° C. in an air atmosphere.
[0028] Table 1 High temperature flexural strength of each embodiment
[0029] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0030] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0031] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing refractory materials from black carbon silicon tailings from phosphogypsum flotation, characterized in that: The method comprises the following steps: (1) Washing the black carbon silicon tailings from the flotation of phosphogypsum with water; (2) After washing, the black carbon silicon tailings are dried in an oven, the dried tailings are mixed with coal gasification slag, and then washed with acid under heating conditions to remove impurities, and then placed in an electric furnace for heating to obtain silicon carbide powder; (3) The silicon carbide powder and magnesia alumina spinel in step (2) are used as raw materials for refractory materials, and a binder is added. The raw materials and the binder are mixed and pressure-formed on a hydraulic press or a friction brick press. After room temperature curing and oven drying, a silicon carbide-magnesia alumina spinel refractory material is obtained.
2. The method according to claim 1, characterized in that The water temperature of the water washing in step (1) is 80-100° C.; the SiO2 content, F content and P2O5 content of the black carbon silicon tailings from the phosphogypsum flotation in step (1) are 50-80wt%, 1-2wt% and 3-10wt%.
3. The method according to claim 1, characterized in that In the step (2), the black carbon silicon tailings from the phosphogypsum flotation after washing are mixed with coal gasification slag, and coke is added, washed with a 5-20wt% sulfuric acid solution at a temperature of 60-80°C, heated to 1800-2200°C, and reacted for 5-10h; The coal gasification slag is the slag remaining after coal is gasified in a gasifier; the C content in the coal gasification slag is 5-20wt%, and the SiO2 content is 40-60wt%; the mass ratio of the dried tailings to the coal gasification slag is 0.5-1.
5.
4. The method according to claim 3, characterized in that Before the heating, one or more of urea, ammonium chloride, ammonium sulfate and ammonium nitrate are added, and the addition amount of one or more of urea, ammonium chloride, ammonium sulfate and ammonium nitrate is 5-10% of the mixed mass of black carbon silicon tailings from phosphogypsum flotation and coal gasification slag.
5. The method according to claim 4, characterized in that After the black carbon silicon slag is mixed with the coal gasification slag, coke in an amount of 20-40% by weight of the mixture of the black carbon silicon slag and the coal gasification slag is added.
6. The method according to claim 1, characterized in that The raw material composition and mass percentage of the unfired refractory material in step (3) are as follows: the silicon carbide powder has a particle size of 0.1-3 mm and a content of 55-70 wt %; The magnesia-alumina spinel has a particle size of 20-90 μm and a content of 20-30 wt%; The alumina is a micro powder with a D50 of 5-10 μm and a content of 2-8 wt%; The metal aluminum powder has a particle size of 35-75 μm and a content of 2-8 wt %.
7. The method according to claim 1, characterized in that The magnesium-aluminum spinel in step (3) can be prepared from secondary aluminum ash acidolysis slag; the secondary aluminum ash acidolysis slag used to prepare the magnesium-aluminum spinel comes from the slag after acidolysis treatment of the main by-product produced in the aluminum smelting and molding process.
8. The method according to claim 1, characterized in that The binder added in step (3) is sodium superpolyphosphate and urea-formaldehyde resin; The addition amount of the binder sodium super polyphosphate and urea-formaldehyde resin is 3-4wt% of the weight of the silicon carbide-magnesium aluminum spinel raw material.
9. The method according to claim 1, characterized in that: In the step (4), the pressure forming is performed by a hydraulic press or a friction brick press; the pressure forming is performed at 130-150 MPa; the room temperature curing time is 18-20 hours; and the oven drying is performed at 150-200° C. for 18-24 hours.
Citation Information
Patent Citations
Nitride-silicon carbide-magnesium aluminate spinel multiphase refractory material product and preparation method thereof
CN111875398A
Unfired silicon carbide-magnesium aluminate spinel refractory material as well as preparation method and product thereof
CN115028455A
Flotation tailing collecting device and working method and application thereof
CN115921127A
Porous coal gasification slag-silicon carbide composite ceramic support and preparation method thereof
CN117142875A
Method for preparing magnesium aluminate spinel from aluminum electrolysis ash
CN117776707A
Cited By
Method for preparing silicon carbide material from coal gasification slag
CN119409195A
A method for preparing silicon carbide materials using coal gasification slag