Low-cost anti-ablation anti-scouring carbon / carbon lining and manufacturing method thereof

By using a three-dimensional prefabrication method and an impregnation-curing carbonization-graphitization process, a porous carbon/carbon liner was prepared and wrapped with an outer fiber insulation layer. This solved the problem of insufficient rigidity of the solid rocket motor nozzle liner at high temperatures and achieved low-cost, high-efficiency ablation and erosion resistance.

CN118978404APending Publication Date: 2024-11-19XIAN YINGLIKE ELECTRIC TECH CO LTD

Patent Information

Application Number
CN202411058525.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing technologies struggle to maintain the rigidity and ablation resistance of solid rocket motor nozzle liners at high temperatures, especially during prolonged operation or under multi-pulse conditions. Traditional materials lose the support of the matrix resin at high temperatures, resulting in softness and failing to meet the requirements for erosion and ablation resistance.

Method used

A three-dimensional preform manufacturing method is adopted. By fitting a three-dimensional preform onto a core mold and embedding a throat liner, combined with impregnation, curing, carbonization and graphitization processes, a porous carbon/carbon liner with a density of 0.6 to 1.2 g/cm3 is prepared. A fiber-wound insulation layer is then wrapped on the outside to form an integrated woven structure.

Benefits of technology

It achieves low-cost and high-efficiency manufacturing of carbon/carbon liners, which have good resistance to ablation and erosion, can maintain stable geometry at high temperatures, reduce carbon fiber ablation rate, improve thermal insulation effect, and prevent throat dimensional deformation and fire penetration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978404A_ABST
    Figure CN118978404A_ABST
Patent Text Reader

Abstract

The invention relates to a low-cost anti-ablation anti-scouring carbon / carbon lining and a manufacturing method thereof, and the manufacturing method comprises the following steps: manufacturing a three-dimensional prefabricated body, and sleeving the three-dimensional prefabricated body on a core mold; inlaying a throat liner on the three-dimensional prefabricated body, and then dipping the throat liner and the core mold; the impregnated prefabricated body and the core mold are cured, and a cured composite component is obtained; and carbonizing and graphitizing the cured composite part in sequence, and separating the core mold to obtain the carbon / carbon lining. The method is low in manufacturing cost and short in manufacturing period, and carbonization and graphitization are completed only through one-time dipping and one-time furnace entering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a low-cost ablation-resistant and erosion-resistant carbon / carbon lining and a manufacturing method thereof. Background Art

[0002] The ablation-resistant and erosion-resistant linings of the convergent and expansion sections of the solid rocket engine nozzle must withstand high-speed erosion of high-temperature flames containing solid and liquid particles up to 4000°C during operation. In the past, the working temperature of the propellant was relatively low, and the ablation-resistant and erosion-resistant linings were mainly formed by winding and heating carbon fiber impregnated cloth tapes. In recent years, in order to adapt to the development of propellant technology, more and more solid rocket engine nozzle linings have begun to be manufactured using the better-performing 2.5D circular woven preform dip curing process. However, due to the ultra-high temperature of carbon fiber reinforced resin-based composites, the resin will quickly decompose and gasify. After working for tens of seconds, only fibers and free carbon will appear within a certain thickness near the fire surface. Especially for endurance engines and multi-pulse engines with longer working cycles, the resin will be "hollowed out" more. The resin-based composite reinforced by the long fiber braid without the support of the matrix resin will be as soft as the preform of the simple fiber braid, and its hardness, that is, the elastic modulus, will drop sharply like a cliff. In severe cases, the throat lining will undergo significant axial displacement, threatening the safety of the engine. In the past, some people have tried to use high-density carbon / carbon materials to make the convergent end and expansion section of the integrated nozzle in order to maintain sufficient rigidity in a high temperature environment. However, for tactical missile rocket engines that need to install steering gear and other equipment on the outside of the nozzle, an insulation layer must be set on the outside of the liner for thermal protection. Due to the high thermal conductivity and low porosity of high-density carbon / carbon materials, when the engine is working, the resin in the insulation layer decomposes rapidly from the inside to the outside, and the generated gas forms a local high pressure on the outside of the liner due to the small number of pores in the liner and the poor discharge channel, which will crack the carbon / carbon liner. TW201325879A1 discloses a "composite pipe with a three-dimensional woven structure with an intermediate lock and a manufacturing method" that shows the characteristics and manufacturing method of the integrated three-dimensional woven preform resin-based nozzle liner, but this liner is not suitable for the 3000-4000℃ combustion temperature of the double-base propellant with aluminum powder added to the long-term solid rocket. The paper "Low-density carbon / carbon composite molding method and its application" published by Wang Taogen and Wang Junshan showed people the basic production method and application scenarios of porous low-density carbon / carbon composite materials, but the performance of its preforms is not competent for the working stress faced by the solid rocket engine nozzle lining. In addition, Zuo Xiangchun's doctoral thesis "One-step preparation of carbon / carbon composite materials" gave a specific method and actual case of using asphalt-based fibers to make carbon-carbon composites in one step, but because the fiber loses too much weight in the process of converting into carbon fiber, the volume density of the carbon / carbon material fiber is too low, the mechanical properties are poor, and the quality is difficult to stabilize. It is also not competent for the low ablation rate and anti-scouring requirements of the convergence and expansion sections of the solid rocket engine nozzle. Xi'an Chaoma CN 101758380A "A method for preparing a wound carbon / carbon tube" shows a technical solution using fiber winding as a carbon-carbon tube reinforcement material, but the carbon / carbon tube produced by this method has weak interlayer bonding and is not suitable for rocket nozzle linings. Summary of the invention

[0003] The object of the present invention is to provide a low-cost ablation-resistant and erosion-resistant carbon / carbon lining and a manufacturing method to solve the above problems.

[0004] To achieve the above object, the present invention adopts the following technical solutions:

[0005] A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner, comprising:

[0006] Making a three-dimensional preform, and fitting the three-dimensional preform onto the core mold;

[0007] The throat liner is inlaid on the three-dimensional preform and then impregnated together with the core mold;

[0008] The impregnated preform and the core mold are cured to obtain a cured composite component;

[0009] The cured composite parts are sequentially carbonized and graphitized, and after the core mold is separated, a variable diameter tubular porous carbon / carbon lining with a density of 0.6 to 1.2 g / cm3 is obtained.

[0010] Further, a three-dimensional preform is manufactured and the three-dimensional preform is mounted on a core mold, including:

[0011] A three-dimensional preform is obtained by performing 2.5D circular weaving with carbon fiber outside a braided core mold, and then the three-dimensional preform is sheathed on a carbonized core mold made of graphite or ceramic.

[0012] Further, the throat liner is inlaid on the three-dimensional preform, and then impregnated together with the core mold, including:

[0013] Resin or asphalt is used as the impregnating resin, the three-dimensional preform together with the core mold and the resin to be impregnated is heated to 80° C., and the preform is impregnated by a vacuum introduction method.

[0014] Furthermore, the impregnated preform and the core mold are cured to obtain a cured composite component, including:

[0015] The preform impregnated with resin, together with the core mold, is wrapped with absorbent cotton and vacuum bag film and placed in an autoclave for curing. The temperature is first quickly raised to 80°C at a rate of 10°C / min, then raised to 120°C at a rate of 2°C / min and kept warm for 30 minutes to allow the phenolic resin to undergo a smooth condensation reaction, and then raised to 170°C at a rate of 2°C / min and kept warm for 1 hour to complete the curing.

[0016] Further, the cured composite component is carbonized, including:

[0017] The cured composite parts were taken out and loaded into a graphitization furnace for carbonization. Under an inert atmosphere, the temperature was raised to 400°C at a rate of 20°C / min, then raised to 450°C at a rate of 5°C / min and kept warm for 30 minutes, and then raised to 500°C at a rate of 5°C / min and kept warm for 10 minutes to complete low-temperature carbonization. Subsequently, high-temperature carbonization was performed by raising the temperature to 1400°C at a rate of 50°C / min and keeping warm for 10 minutes under an inert atmosphere.

[0018] Further, the cured composite component is graphitized, including: heating to 2000-2500° C. at a rate of 50° C. / min under an inert atmosphere and keeping the temperature for more than 15 minutes, and then naturally cooling to room temperature.

[0019] Furthermore, the throat liner made of high-density carbon / carbon material is pre-set on a woven, carbonized, and graphitized core mold made of graphite, and an inner liner preform with an integrated woven 2.5D circular weave structure is performed outside the preform, so that the throat liner is embedded in the preform.

[0020] Furthermore, when the manufacturing process of the lining does not include high-temperature graphitization, if the maximum temperature is not higher than 1400°C, a throat lining made of high-temperature resistant metal material can be used for integrated weaving; if the manufacturing process of the lining only involves carbonization at a maximum temperature below 900°C, a throat lining made of tungsten-infiltrated copper material can be used for integrated weaving.

[0021] Furthermore, the outer side of the carbon / carbon liner is wrapped with a fiber-wound insulation layer.

[0022] A low-cost ablation-resistant and erosion-resistant carbon / carbon liner is prepared based on a low-cost ablation-resistant and erosion-resistant carbon / carbon liner manufacturing method.

[0023] Compared with the prior art, the present invention has the following technical effects:

[0024] The invention has low manufacturing cost and short manufacturing cycle, and only one impregnation and one furnace entry are required to complete carbonization and graphitization.

[0025] The carbon / carbon lining of the present invention has low density and many pores, which is conducive to the discharge of thermal decomposition gas of the resin-based thermal insulation composite material outside the nozzle. The discharged gas not only limits the temperature of the pyrolysis interface but also effectively cools the carbon fiber of the lining and drives away the oxygen in the flame attempting to enter the lining, further reducing the ablation rate of the carbon fiber.

[0026] The strength and modulus of the liner at high temperature of the present invention are much higher than those of the resin-based composite material, and the liner can maintain a stable geometric shape when working at high temperature and for a long time.

[0027] The present invention adopts an embedded throat liner and an external fiber-wound insulation layer, which can ensure the stability of the throat size and the reliability of operation, and can also increase the thermal resistance of the insulation layer and improve the thermal insulation effect.

[0028] The convergence section and expansion section liner preforms of the integrated braided embedded throat liner of the present invention can completely prevent the occurrence of fire penetration, and no cracks will appear after multiple high and low temperature alternations. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of a core mold used in the liner of the present invention and a manufacturing process thereof;

[0030] Figure 2 It is a schematic diagram of the inner liner with an embedded throat liner and a wrapped insulation layer of the present invention;

[0031] Among them: 1 - lining, 2 - core mold, 3 - throat lining, 4 - insulation layer. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with the accompanying drawings:

[0033] See also Figure 1 to Figure 2 Embodiment 1: The present invention provides a method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner, comprising:

[0034] Making a three-dimensional preform, and fitting the three-dimensional preform onto the core mold;

[0035] The throat liner is inlaid on the three-dimensional preform and then impregnated together with the core mold;

[0036] The impregnated preform and the core mold are cured to obtain a cured composite component;

[0037] The cured composite parts are carbonized and graphitized in sequence, and the carbon / carbon lining is obtained after the core mold is separated.

[0038] Example 2, a method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner, see Figure 1 .

[0039] First, carbon fiber is woven in 2.5D circular weave outside a braided core mold to obtain a three-dimensional preform with a composite design requirement for inner cavity contour and thickness; then the preform is mounted on a carbonized core mold made of graphite, ceramic or heat-resistant metal; a resin or asphalt with a high carbon residue rate after pyrolysis is used as an impregnation resin, the preform together with the core mold and the resin to be impregnated is heated to 80°C, and the preform is impregnated by a vacuum introduction method;

[0040] The preform impregnated with resin and the core mold are covered with absorbent cotton and vacuum bag film and placed in an autoclave for curing. The temperature is first quickly raised to 80°C at a rate of 10°C / min, then raised to 120°C at a rate of 2°C / min and kept warm for 30 minutes to allow the phenolic resin to undergo a slow polycondensation reaction, and then raised to 170°C at a rate of 2°C / min and kept warm for 1 hour;

[0041] After the furnace is cooled to near room temperature, the cured composite parts are taken out and loaded into the graphitization furnace for carbonization and graphitization. In an inert atmosphere, the temperature is increased to 400°C at a rate of 20°C / min, then increased to 450°C at a rate of 5°C / min and kept warm for 30 minutes, then increased to 500°C at a rate of 5°C / min and kept warm for 10 minutes to complete low-temperature carbonization, followed by high-temperature carbonization, and then increased to 1400°C at a rate of 50°C / min and kept warm for 10 minutes in an inert atmosphere. Finally, graphitization is performed: in an inert atmosphere, the temperature is increased to 2400°C at a rate of 50°C / min and kept warm for 5 minutes, and then naturally cooled to room temperature in 12 hours;

[0042] After the furnace is opened, the core mold is separated from the carbon / carbon composite part and the carbon / carbon composite blank is machined to the designed size. In order to slow down the decomposition process of the resin during the carbonization process, the temperature rise rate of the carbonization process should be as low as possible in the temperature range from the beginning decomposition temperature of the resin to the complete decomposition temperature.

[0043] Example 3: A low-cost method for manufacturing ablation-resistant and erosion-resistant carbon / carbon lining, see Figure 1 .

[0044] First, carbon fiber is used for 2.5D circular weaving outside the braided core mold to obtain a three-dimensional preform with the composite design requirements of the inner cavity contour; then the preform is set on a carbonized core mold made of graphite, ceramic or heat-resistant metal; the preform, together with the core mold and the asphalt to be impregnated, is placed in the heald frame pressure impregnation tank, and the asphalt is impregnated under high pressure at 10MPa and 200℃; the preform impregnated with asphalt is placed in a graphitization furnace, and carbonized at 10MPa and 500℃ under an inert atmosphere. After carbonization, the temperature is raised to 2400℃ under an inert atmosphere for graphitization. The shallow cross-bend structure of the 2.5D circular woven preform makes the layers interlocked but not penetrated inside and outside, which greatly improves the interlayer bonding strength without increasing the thermal conductivity between the layers. It does not delaminate or fall off in pieces under the scouring of high-temperature and high-speed gas front, and can effectively prevent heat from being transferred radially outward.

[0045] Example 4: A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner and a thermal insulation layer of an integrated braided preform containing a throat liner, see Figure 1 , Figure 2 .

[0046] The preform weaving adopts an axially butted spliced ​​graphite braided core mold. Before weaving, a high-density carbon / carbon throat liner is set at the waist of the core mold, and then carbon fiber is used to perform 2.5D circular weaving outside the braided core mold to obtain a three-dimensional preform with a composite design requirement for the inner cavity contour; the preform together with the core mold and the resin to be impregnated are preheated, and polyacetylene resin is impregnated by vacuum introduction; the preform impregnated with resin is placed in a graphitization furnace for low-temperature carbonization according to the thermal decomposition temperature of polyacetylene, then high-temperature carbonization, and finally high-temperature graphitization. After cooling, the inner lining contour is machined to meet the design requirements, and then the outer side is wound with a high-silica cloth tape pre-impregnated with barium phenolic to a certain thickness, or high-silica fiber or quartz fiber is wet-wound, or pre-impregnated high-silica fiber or quartz fiber is dry-wound; it is placed in an air pressure autoclave or a hydraulic autoclave for curing, and after being taken out of the furnace, it is machined to the design size.

[0047] The nozzle made in this way can be used for long-term endurance engines and multi-pulse engines. Its lining will not deform due to long-term high heat during operation, nor will it have gaps due to multiple high and low temperature cycles like traditional bonded splicing linings. The multi-void characteristics of the low-density carbon / carbon lining also allow the gas generated by the thermal decomposition process of the resin of the insulation layer to pass through the lining smoothly and enter the flame, avoiding the local excessive pressure on the outside of the lining. On the one hand, the thermal decomposition of the insulation layer resin hinders the speed of heat transfer to the outside; on the other hand, the pyrolyzed gas will take away a lot of heat from the higher temperature lining when passing through the lining, reducing the temperature rise of the lining, and these gases can also prevent the oxygen in the flame from penetrating into the lining, reducing the ablation of the lining carbon / carbon material. The normal thermal resistance of the fiber-wound insulation layer is no less than that of the cloth tape winding, and the mechanical properties are far better than the cloth tape winding, and the manufacturing cost is lower.

[0048] The above is only the most typical specific implementation of the present invention, but the protection scope of the present invention is not limited to this. Due to space limitations, the production steps of the traditional process used are not described in detail, but it does not mean that the omitted process steps do not exist. The listed data are only used to describe the working principle of the present invention and do not represent necessary values. Any technician familiar with composite material manufacturing and related fields can easily think of equivalent changes within the technical scope disclosed by the present invention, which should be covered within the scope of the claims of the present invention.

Claims

1. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner, characterized in that: include: Making a three-dimensional preform, and fitting the three-dimensional preform onto the core mold; The throat liner is inlaid on the three-dimensional preform and then impregnated together with the core mold; The impregnated preform and the core mold are cured to obtain a cured composite component; The cured composite parts are carbonized and graphitized in sequence, and the density is 0.6-1.2 g / cm after the core mold is separated. 3 Variable diameter tubular porous carbon / carbon liner.

2. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 1, characterized in that: Making a three-dimensional preform and fitting the three-dimensional preform on a core mold, including: A three-dimensional preform is obtained by performing 2.5D circular weaving with carbon fiber outside a braided core mold, and then the three-dimensional preform is sheathed on a carbonized core mold made of graphite or ceramic.

3. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 1, characterized in that: The throat liner is inlaid on the three-dimensional preform and then impregnated together with the core mold, including: Resin or asphalt is used as the impregnating resin, the three-dimensional preform together with the core mold and the resin to be impregnated is heated to 80° C., and the preform is impregnated by a vacuum introduction method.

4. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 1, characterized in that: The impregnated preform and the core mold are cured to obtain a cured composite component, including: The preform impregnated with resin, together with the core mold, is wrapped with absorbent cotton and vacuum bag film and placed in an autoclave for curing. The temperature is first quickly raised to 80°C at a rate of 10°C / min, then raised to 120°C at a rate of 2°C / min and kept warm for 30 minutes to allow the phenolic resin to undergo a smooth condensation reaction, and then raised to 170°C at a rate of 2°C / min and kept warm for 1 hour to complete the curing.

5. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 4, characterized in that: Carbonization of cured composite parts, including: The cured composite parts were taken out and loaded into a graphitization furnace for carbonization. Under an inert atmosphere, the temperature was raised to 400°C at a rate of 20°C / min, then raised to 450°C at a rate of 5°C / min and kept warm for 30 minutes, and then raised to 500°C at a rate of 5°C / min and kept warm for 10 minutes to complete low-temperature carbonization. Subsequently, high-temperature carbonization was performed by raising the temperature to 1400°C at a rate of 50°C / min and keeping warm for 10 minutes under an inert atmosphere.

6. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 4, characterized in that: The cured composite component is graphitized, including: heating to 2000-2500° C. at a rate of 50° C. / min under an inert atmosphere and keeping the temperature for more than 15 minutes, and then naturally cooling to room temperature.

7. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 1, characterized in that: The throat liner made of high-density carbon / carbon material is pre-placed on a woven, carbonized, and graphitized core mold made of graphite, and an inner liner preform of a 2.5D circular weave structure is integrally woven outside the core mold, so that the throat liner is embedded in the preform.

8. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 7, characterized in that: When the manufacturing process of the lining does not include high-temperature graphitization, if the maximum temperature is not higher than 1400°C, a throat lining made of high-temperature resistant metal material is used for integrated weaving; if the manufacturing process of the lining only involves carbonization at a maximum temperature below 900°C, a throat lining made of tungsten-copper infiltrated material is used for integrated weaving.

9. A method for manufacturing a low-cost ablation-resistant and erosion-resistant carbon / carbon liner according to claim 1, characterized in that: The carbon / carbon liner is wrapped with fiber-wound insulation on the outside.

10. A low-cost anti-ablation and anti-erosion carbon / carbon liner, characterized in that: It is prepared based on the low-cost ablation-resistant and erosion-resistant carbon / carbon lining manufacturing method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Nozzle with non-weft cloth punched throat liner

    CN109184959A

  • Preparation method of ultrahigh-temperature ceramic modified C / C composite material

    CN110803942A

  • Rapid preparation method of C / SiC composite material engine nozzle

    CN112358298A

  • Woven round tube and weaving method thereof

    CN114606622A

  • High-purity light carbon fiber / carbon composite thermal field material and preparation method thereof

    CN115353403A

Cited By

  • Solid rocket nozzle capable of repeatedly igniting and engine

    CN119102925A