Erythroryl modified polymer as well as preparation method and coating thereof
The erythross red-based modified polymer is formed by reacting and copolymerizing erythross red-based derivatives with amino bromide, which solves the problems of the preparation complexity and insufficient antibacterial performance of existing photocatalytic antibacterial coatings, and achieves efficient bacterial killing and coating hardness increase.
Patent Information
- Application Number
- CN202411064894.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing photocatalytic antibacterial coating preparation process is complex, the raw materials are difficult to obtain, the cost is high and easy to precipitate, and the application field is limited, making it difficult to effectively improve antibacterial performance and hardness.
The reaction of erythrosin derivatives and amino bromides is used to form amino erythrosin derivatives, and carboxy groups are introduced through copolymerization reaction to form erythrosin modified polymers, which improves antibacterial properties through amidation reaction, and introduces branched chains. Double bonds form a stable antibacterial coating, improving the hardness and stability of the coating.
It significantly improves the antibacterial properties of erythromycated red-based modified polymers and the hardness and stability of the coating, and achieves efficient bacterial killing and anti-fouling properties, and is suitable for a variety of substrate materials.
Smart Images

Figure CN118978625A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of antibacterial materials, and in particular to an erythrosine-modified polymer and a preparation method and a coating thereof. Background Art
[0002] Bacterial infection and bacterial resistance are one of the serious global public health problems, which has caused many problems in many fields such as healthcare, food preservation and public health. Although antibiotic treatment is a common means to fight bacterial infections, the emergence and spread of drug-resistant strains are gradually weakening the effectiveness of traditional antibiotics.
[0003] In recent years, photodynamic therapy (PDT) has attracted much attention due to its targeted selectivity, remote controllability, minimally invasive or non-invasiveness, and biosafety in normal tissues. It relies on the use of photosensitizers (PS). Under light, PS quickly forms its triplet excited state and then transfers to the ground state (triplet) molecular oxygen to generate ROS, including hydroxyl radicals and singlet oxygen. These ROS destroy some biomolecules such as proteins, lipids and nucleic acids through oxidation mechanisms, leading to the dissolution of bacterial membranes and killing bacteria.
[0004] At present, the reported photocatalytic antibacterial coatings have very obvious disadvantages, such as complex preparation process, difficult to obtain raw materials, high cost, easy precipitation, and limited application areas. Summary of the invention
[0005] The main purpose of the invention is to provide an erythrosine-modified polymer and a preparation method and a coating thereof, aiming to improve the hardness and antibacterial performance of the antibacterial coating.
[0006] To achieve the above object, the present invention provides a method for preparing an erythrosin-modified polymer, comprising the following steps: S10. Mixing the erythrosine derivative, the amino bromide and the solvent, heating the mixture to cause an amination reaction to obtain an aminoerythrosine derivative; S20. mixing the first monomer and the second monomer, causing a copolymerization reaction to occur, to obtain a copolymer, wherein the first monomer contains a carboxyl group and a carbon-carbon double bond, and the second monomer contains a double bond and a halogenated alkyl group connected to the double bond; S30. The copolymer is subjected to an elimination reaction to remove the hydrogen halide to obtain a branched copolymer having double bonds; S40. Mixing the aminoerythrosine derivative with the copolymer having double bonds in the side chains, causing an amidation reaction, and obtaining the erythrosine-modified polymer.
[0007] In one embodiment, in step S10, the erythrosine derivative comprises erythrosine B sodium salt; and / or, Aminobromides include 3-bromopropylamine hydrobromide; and / or, The solvent includes any one of dimethylformamide and dimethyl sulfoxide.
[0008] In one embodiment, in step S10, the molar ratio of the erythrosine derivative to the amino bromide is 1:(1-2), wherein the concentration of the erythrosine derivative in the solvent is 0.01-0.1 mol / L.
[0009] In one embodiment, in step S10, the heating temperature is 70-90° C.; and / or, In step S10, the heating time is 6 to 8 hours.
[0010] In one embodiment, the first monomer includes acrylic acid, and the second monomer includes 5-bromo-1-pentene.
[0011] In one embodiment, step S20 further includes the following steps: The first monomer, the second monomer and the third monomer are mixed and copolymerized to obtain a copolymer, wherein the first monomer contains a carboxyl group and a carbon-carbon double bond, the second monomer contains a carbon-carbon double bond and a halogenated alkyl connected to the double bond; and the third monomer contains a carbon-carbon double bond and a polyethylene glycol group.
[0012] In one embodiment, the first monomer is acrylic acid, the second monomer is 5-bromo-1-pentene, and the third monomer is polyethylene glycol methacrylate.
[0013] In one embodiment, in step S20, the mass ratio of the first monomer, the second monomer, and the third monomer is 1:(5-9):(0-4).
[0014] The present invention also provides an erythrosin-based modified polymer, which is prepared according to the above-mentioned preparation method of the erythrosin-based modified polymer.
[0015] The present invention also provides a coating, comprising an erythrin-modified polymer and a free radical photoinitiator, wherein the erythrin-modified polymer is the erythrin-modified polymer as described above.
[0016] The technical solution of the present invention adopts an erythrosine derivative to react with an amino bromide to obtain an aminoerythrosine derivative, and at the same time, introduces a carboxyl group into a copolymer so that the erythrosine derivative can undergo an amidation reaction with the carboxyl group, so as to introduce an erythrosine group into the copolymer to obtain an erythrosine-based modified polymer, so as to improve the antibacterial property of the erythrosine-based modified polymer; and introduces double bonds on the side chains so that the obtained erythrosine-based modified polymers can undergo an addition polymerization reaction to form a stable antibacterial coating through cross-linking, thereby improving the hardness and stability of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 A flow chart of the method for preparing the erythrosin-based modified polymer provided by the present invention; Figure 2 A chemical flow chart of the method for preparing the erythrosin-based modified polymer provided by the present invention; Figure 3 The mass spectrum of the erythrin-modified polymer provided in Example 1 of the present invention; Figure 4 This is a graph showing the static water contact angle experimental results of the erythrosine-based photocatalytic antibacterial and antifouling coating provided in Examples 7 to 8 of the present invention.
[0019] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION
[0020] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.
[0021] It should be noted that, in the embodiments, those without specifying specific conditions are carried out according to normal conditions or conditions recommended by the manufacturer. Those without specifying the manufacturer of reagents or instruments used are conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, and "A and / or B" is taken as an example, including schemes A, B, or A and B that meet the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work, all belong to the scope of protection of the present invention.
[0022] At present, the reported photocatalytic antibacterial coatings have very obvious disadvantages, such as complex preparation process, difficult to obtain raw materials, high cost, easy precipitation, and limited application areas.
[0023] For this reason, please see Figure 1 and Figure 2 The present invention provides a method for preparing an erythrosine-modified polymer, comprising the following steps: S10. mixing an erythrosine derivative, an amino bromide and a solvent, heating them to cause an amination reaction, and obtaining an aminoerythrosine derivative; S20. mixing a first monomer and a second monomer, causing a copolymerization reaction, and obtaining a copolymer, wherein the first monomer contains a carboxyl group and a carbon-carbon double bond, and the second monomer contains a double bond and a halogenated alkyl connected to the double bond; S30. subjecting the copolymer to an elimination reaction, removing hydrogen halide, and obtaining a copolymer with a branched chain having a double bond; S40. mixing the aminoerythrosine derivative and the copolymer with a branched chain having a double bond, causing an amidation reaction, and obtaining the erythrosine-modified polymer.
[0024] The technical solution of the present invention adopts an erythrosine derivative to react with an amino bromide to obtain an aminoerythrosine derivative, and at the same time, introduces a carboxyl group into a copolymer so that the erythrosine derivative can undergo an amidation reaction with the carboxyl group, so as to introduce an erythrosine group into the copolymer to obtain an erythrosine-based modified polymer, so as to improve the antibacterial property of the erythrosine-based modified polymer; and introduces double bonds on the side chains so that the obtained erythrosine-based modified polymers can undergo an addition polymerization reaction to form a stable antibacterial coating through cross-linking, thereby improving the hardness and stability of the coating.
[0025] After being excited under light conditions, the erythrosine-based photosensitizer can react with H 2 O or O 2 Reactive oxygen species (ROS) are generated by the reaction. ROS mainly include superoxide anions (O 2 •− ), singlet oxygen ( 1 O 2 ), hydrogen peroxide (H 2 O 2 ), etc. These ROS with strong oxidative ability can oxidize organic components such as bacterial proteins and deoxyribonucleic acid, affect bacterial metabolism and cause bacterial membrane perforation, thus leading to bacterial death.
[0026] In one embodiment, in step S10, the erythrosine derivative includes erythrosine B sodium salt; and / or, the amino bromide includes 3-bromopropylamine hydrobromide; and / or, the solvent includes any one of dimethylformamide and dimethyl sulfoxide.
[0027] The technical solution of the present invention adopts erythrosin B sodium salt to improve the reaction activity of erythrosin B sodium salt and amino bromide; adopts 3-bromopropylamine hydrobromide to improve the reaction activity of erythrosin derivatives and 3-bromopropylamine hydrobromide; and selects dimethylformamide (DMF) or dimethyl sulfoxide (DMSO) as a solvent, which not only ensures the full dissolution and uniform distribution of reactants, but also accelerates the progress of amination reaction through its unique solvent properties, effectively shortens the reaction time, and improves the selectivity and conversion rate of the reaction.
[0028] In one embodiment, in step S10, the molar ratio of the erythrosine derivative to the amino bromide is 1:(1-2), wherein the concentration of the erythrosine derivative in the solvent is 0.01-0.1 mol / L.
[0029] The technical solution of the present invention ensures efficient amination reaction by adjusting the molar ratio of erythrosine derivatives to amino bromide to 1:(1-2), and a higher amount of amination reagent (1-2 molar ratio of erythrosine) not only promotes the complete reaction and reduces the residual unreacted raw materials, but also promotes the formation of the target product aminoerythrosine derivative through the regulation of dynamic equilibrium, thereby significantly improving the yield of the product and the economy of the reaction; preferably, the molar ratio of erythrosine derivatives to amino bromide is 1:1.5; by adjusting the concentration of erythrosine derivatives in the solvent to 0.01-0.1 mol / L, this concentration range effectively avoids the slow reaction rate caused by too low concentration and the side reaction or competitive reaction problems caused by too high concentration, and the appropriate concentration is not only conducive to the effective collision between reactant molecules, but also promotes the uniform formation of products and reduces the generation of by-products.
[0030] In one embodiment, in step S10, the heating temperature is 70-90°C; and / or, in step S10, the heating time is 6-8 hours.
[0031] The technical solution of the present invention promotes the reaction of erythrosine derivatives with amino bromides to generate aminoerythrosine by adjusting the heating temperature and / or duration, without causing excessive pyrolysis or side reactions; preferably, the heating temperature is 80°C and the heating duration is 7 h.
[0032] In one embodiment, the first monomer includes acrylic acid, and the second monomer includes 5-bromo-1-pentene.
[0033] The technical solution of the present invention adopts acrylic acid and 5-bromo-1-pentene to undergo copolymerization reaction to obtain a copolymer, wherein acrylic acid can provide a carboxyl group to facilitate an amidation reaction with aminoerythrosine, and 5-bromo-1-pentene can provide a brominated alkyl group to facilitate an addition reaction to form a double bond, thereby allowing the generated copolymers with double bonds in the side chains to be cross-linked with each other, thereby improving the hardness of the coating formed by the cross-linking and improving the stability of the coating.
[0034] In one embodiment, step S20 also includes the following steps: mixing a first monomer, a second monomer, and a third monomer to undergo a copolymerization reaction to obtain a copolymer, wherein the first monomer contains a carboxyl group and a carbon-carbon double bond, the second monomer contains a carbon-carbon double bond and a halogenated alkyl group connected to the double bond; and the third monomer contains a carbon-carbon double bond and a polyethylene glycol group.
[0035] The technical solution of the present invention adopts a third monomer containing a carbon-carbon double bond and a polyethylene glycol group, wherein the carbon-carbon double bond enables the third monomer to participate in the polymerization reaction, and copolymerizes with the first monomer and the second monomer to form a copolymer; in the polyethylene glycol group, the prepolymer having a long branched chain of polyethylene glycol (PEG) has excellent anti-bacterial adhesion ability and adhesion, because the hydration layer formed by the hydroxyl group in PEG can effectively prevent bacteria from adhering to the matrix, and the long-chain PEG molecular brush also helps to remove adhered bacteria.
[0036] In one embodiment, the first monomer is acrylic acid, the second monomer is 5-bromo-1-pentene, and the third monomer is polyethylene glycol methacrylate.
[0037] The technical solution of the present invention adopts polyethylene glycol methacrylate as the third monomer, which has a simple molecular structure and is easy to obtain, and is helpful for removing adherent bacteria. In addition, in one embodiment of the present invention, the first monomer, the second monomer and the third monomer are also mixed with a thermal initiator. By adopting the thermal initiator, a polymerization reaction can occur under heating conditions, so that each monomer can be fully mixed before heating to improve the uniformity of the product. Specifically, in one embodiment of the present invention, the thermal initiator is azobisisobutyronitrile.
[0038] In one embodiment, in step S2, the mass ratio of the first monomer, the second monomer, and the third monomer is 1:(5-9):(0-4).
[0039] The technical solution of the present invention can adjust the proportion of each monomer in the copolymer intermediate by adjusting the mass ratio of the first monomer, the second monomer and the third monomer, thereby adjusting the crosslinking ability and the anti-adhesion bacteria rate of the copolymer, and then changing the hardness and anti-adhesion bacteria rate of the coating formed by crosslinking.
[0040] The present invention also provides an erythrosin-based modified polymer, which is prepared according to the above-mentioned preparation method of the erythrosin-based modified polymer.
[0041] Since the erythrosin-based modified polymer adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0042] The present invention also provides a coating, comprising an erythrin-modified polymer and a free radical photoinitiator, wherein the erythrin-modified polymer is the erythrin-modified polymer as described above.
[0043] Since the present coating adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0044] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0045] Example 1 This embodiment provides an erythrosin-modified polymer, the preparation method of which comprises the following steps: Step 1: Add 891.8 mg of erythrosine (ER) B sodium salt (1 mmol), 5 mL of dimethylformamide (DMF) and 328.4 mg of 3-bromopropylamine hydrobromide (1.5 mmol) to a 50 mL round-bottom flask and place the apparatus under nitrogen protection. Keep the reaction mixture in the dark at 80 °C and continue stirring for 7 h. After the reaction stops, a mixture containing ER and ER-NH 2 The mixture was poured into 40 mL of a mixture of ether and deionized water (v 乙醚 / v 水 =1:1) to obtain ER-NH 2 After washing with a mixture of ether and deionized water for several times and centrifuging, the precipitate was collected and dried in a vacuum for 24 h to obtain ER-NH 2 (Brick red powder).
[0046] Step 2: Add acrylic acid, 5-bromo-1-pentene, and polyethylene glycol methacrylate in a ratio of 1:9:0 (200 mg:1800 mg:0 mg) into a 50 mL eggplant-shaped bottle. The amount of thermal initiator azobisisobutyronitrile is 20 mg, and 20 mL of anhydrous ethanol is added to the eggplant-shaped bottle as the reaction solvent. Then, in N 2The reaction mixture was slowly heated to 60 °C in an atmosphere of , stirred and refluxed for 12 hours, and then the reaction was terminated. After the reaction system was cooled, part of the solvent was removed by rotary evaporation. Subsequently, a large amount of n-hexane was added to the system to obtain a white precipitate, which was collected and vacuum dried overnight to obtain a copolymer product.
[0047] Step 3: Dissolve the copolymer obtained in the previous step in 40 mL of anhydrous ethanol to prepare a solution of a certain concentration, slowly add it and 2 M sodium hydroxide solution into a three-necked flask with a stirrer, slowly heat to 95°C, stir and reflux for 4 hours, and then end the reaction. After the reaction system is cooled, add 2 M hydrochloric acid to the system to neutralize the excess sodium hydroxide and adjust the pH to around 7.0. Separate and purify the product by extraction and distillation. Finally, a copolymer product (AMP) with double bonds on the side chains is obtained.
[0048] Step 4: Weigh 500 mg of the copolymerized product AMP, add it to 40 mL of dimethyl sulfoxide, and stir vigorously until it is completely dissolved. 2 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDC) (19 mg, 0.1 mM) and N-hydroxysuccinimide (NHS) (23 mg, 0.2 mM) were added thereto under an atmosphere of 4% CO, and the pH value of the reaction solution was adjusted to 5.5 with 2 M hydrochloric acid and 2 M sodium hydroxide, and the reaction was stirred for 1 hour. Finally, 100 mg of ER-NH 2 , and the pH value of the reaction solution was adjusted to 7.5. After 12 hours of reaction, the pH was adjusted to about 7.0 to terminate the reaction. Use a 3500 Da dialysis membrane to dialyze to remove dimethyl sulfoxide. The specific dialysis process is to dialyze in deionized water for 2 days, and replace the dialysis solution every 2 hours. After the dialysis is completed, the mixed solution is centrifuged to collect the precipitate, and the deionized water is washed several times to remove impurities. The precipitate is dissolved with a small amount of dichloromethane, and insoluble impurities are removed after high-speed centrifugation. After the solution is rotary evaporated to remove the solvent, a prepolymer containing ER is obtained, which is an erythrin-modified polymer, named AMPE.
[0049] Example 2 This embodiment provides an erythrosin-modified polymer, the preparation method of which is similar to that of Example 1, except that: The masses of acrylic acid, 5-bromo-1-pentene, and polyethylene glycol methacrylate in step 2 are 200 mg: 1400 mg: 400 mg, respectively, and the mass ratio thereof is 1:7:2.
[0050] Example 3 This embodiment provides an erythrosin-modified polymer, the preparation method of which is similar to that of Example 1, except that: The masses of acrylic acid, 5-bromo-1-pentene, and polyethylene glycol methacrylate in step 2 are 200 mg: 1000 mg: 800 mg, respectively, and the mass ratio thereof is 1:5:4.
[0051] Example 4 This embodiment provides an erythrosine-based photocatalytic antibacterial antifouling coating, the preparation method of which comprises the following steps: AMPE and 20 mg TPO in Example 1 were added to a tetrahydrofuran solution and ultrasonicated until completely dissolved to prepare a solution with a polymer content of 30 mg / mL. The solution was then deposited on a glass substrate by spin coating at 2000 rpm for 20 seconds. After UV irradiation for 10 min, an erythrosine (ER)-based photocatalytic antibacterial and antifouling coating was obtained.
[0052] Example 5 This embodiment provides an erythrosine-based photocatalytic antibacterial antifouling coating, the preparation method of which comprises the following steps: AMPE and 20 mg TPO in Example 2 were added to a tetrahydrofuran solution and ultrasonicated until completely dissolved to prepare a solution with a polymer content of 30 mg / mL. The solution was then deposited on a glass substrate by spin coating at 2000 rpm for 20 seconds. After UV irradiation for 10 min, an erythrosine (ER)-based photocatalytic antibacterial and antifouling coating was obtained.
[0053] Example 6 This embodiment provides an erythrosine-based photocatalytic antibacterial antifouling coating, the preparation method of which comprises the following steps: AMPE and 20 mg TPO in Example 3 were added to a tetrahydrofuran solution and ultrasonicated until completely dissolved to prepare a solution with a polymer content of 30 mg / mL. The solution was then deposited on a glass substrate by spin coating at 2000 rpm for 20 seconds. After UV irradiation for 10 min, an erythrosine (ER)-based photocatalytic antibacterial and antifouling coating was obtained.
[0054] Example 7 This embodiment provides an erythrosine-based photocatalytic antibacterial antifouling coating, and its preparation method is similar to that of Example 4, except that the glass base is replaced by a PVC base.
[0055] Example 8 This embodiment provides an erythrosine-based photocatalytic antibacterial antifouling coating, the preparation method of which is similar to that of embodiment 4, except that the glass base is replaced by Al 2 O 3 Base.
[0056] Comparative Example 1 This comparative example provides an erythrosin-modified polymer, the preparation method of which is similar to that of Example 1, except that: In step 2, the masses of acrylic acid, 5-bromo-1-pentene, and polyethylene glycol methacrylate are 200 mg:0:800 mg, respectively, and the mass ratio thereof is 1:0:4.
[0057] Comparative Example 2 This comparative example provides an erythrosin-modified polymer, and its preparation method is similar to that of Example 1, except that: step 4 is removed, and the AMPE in step 5 is replaced by the AMP prepared in step 3.
[0058] Comparative Example 3 This comparative example provides an erythrosine-based photocatalytic antibacterial antifouling coating, and the preparation method thereof comprises the following steps: AMPE and 20 mg TPO in Comparative Example 1 were added to a tetrahydrofuran solution and ultrasonicated until completely dissolved to prepare a solution with a polymer content of 30 mg / mL. The solution was then deposited on a glass substrate by spin coating at 2000 rpm for 20 seconds. After UV irradiation for 10 min, an erythrosine (ER)-based photocatalytic antibacterial and antifouling coating was obtained.
[0059] Comparative Example 4 This comparative example provides an erythrosine-based photocatalytic antibacterial antifouling coating, and the preparation method thereof comprises the following steps: AMPE and 20 mg TPO in Comparative Example 2 were added to a tetrahydrofuran solution and ultrasonicated until completely dissolved to prepare a solution with a polymer content of 30 mg / mL. The solution was then deposited on a glass substrate by spin coating at 2000 rpm for 20 seconds. After UV irradiation for 10 min, an erythrosine (ER)-based photocatalytic antibacterial and antifouling coating was obtained.
[0060] Performance Testing The erythrin-modified polymer prepared in Example 1 was subjected to mass spectrometry analysis.
[0061] Mass spectra such as Figure 3 As shown, according to Figure 3 It is not difficult to find that: 1649 cm -1 The absorption peak at is attributed to the stretching vibration of -C=O- on the benzene ring. Compared with the raw material, ER-NH 2 At 1715cm -1 A new absorption peak appears at , which is attributed to the stretching vibration of ROC=O. This indicates that ER-NH 2 has been successfully synthesized.
[0062] 3014cm -1 、1715 cm-1 and 1640 cm -1 The absorption peak at corresponds to the stretching vibration of -CH on the terminal C=C, the stretching vibration of -NC=O and the bending vibration of C=O. This indicates the successful formation of the double bond and the 2 Successful grafting.
[0063] The erythrosine (ER)-based photocatalytic antibacterial and antifouling coatings (about 20 micrometers thick) obtained in Examples 4 to 6 and Comparative Examples 3 to 4 were tested for hardness, adhesion, flexibility, antibacterial properties, and antifouling properties.
[0064] The hardness is tested according to the method described in the national standard GB / T6739-2006 "Determination of paint film hardness by pencil method for paints and varnishes".
[0065] The flexibility is tested according to the method described in the national standard GB / T 1731-2020 "Determination of paint film flexibility". The adhesion is tested according to the method described in the national standard GB / T9286-1998 "Scratch test for paints and varnishes".
[0066] For the antibacterial performance test, 1×106 CFU / mL of Escherichia coli liquid was selected for use. The sample was placed in a 24-well plate, 1980 μL of PBS buffer was added, and then 20 μL of the bacterial liquid was added and mixed evenly. Under visible light irradiation, 50 μL of the liquid was taken to coat the plate at 60 min, and the bactericidal ability of the coating was observed after incubation at 37°C for 12 h.
[0067] For the antifouling performance (anti-bacterial adhesion) test, we used 1×107 CFU / mL of Escherichia coli liquid. 30 μL of the liquid was placed on an untreated glass plate and a coated glass plate, covered with a polyethylene film, and co-cultured at 37 °C for 4 h. After gently washing with PBS, the sample was transferred to a 2 mL PBS buffer sterilized tube, and after ultrasonication for 2 min, 50 μL of the liquid was applied to the plate, and the anti-bacterial adhesion ability of the coating was observed after culturing at 37 °C for 12 h.
[0068] Table 1 Test results of erythrosine red (ER)-based photocatalytic antibacterial and antifouling coatings
[0069] As can be seen from Table 1, the hardness of the prepolymers with double bonds introduced (Examples 4, 5, 6 and Comparative Example 4) is significantly higher than that of the prepolymers without double bonds introduced (Comparative Example 3). This is because the double bonds further react and solidify under the conditions of light and initiator to increase the crosslinking density and hardness. Prepolymers with long PEG branches have excellent anti-bacterial adhesion and adhesion, because the hydration layer formed by the hydroxyl groups in PEG can effectively prevent bacteria from adhering to the matrix, and the long-chain PEG molecular brushes also help to remove adherent bacteria; At the same time, compared with the prepolymer without erythrosine, the prepolymer grafted with erythrosine has excellent antibacterial properties.
[0070] The static water contact angle test was conducted on the erythrosine-based photocatalytic antibacterial antifouling coatings provided in Examples 7 to 8. The experimental results are as follows: Figure 4 As shown, the test object in (a) is a PVC substrate, the test object in (b) is a PVC substrate coated with the erythrosine-based photocatalytic antibacterial antifouling coating provided in Example 7, and the test object in (c) is an Al 2 O 3 The test object in (d) is Al coated with the erythrosine-based photocatalytic antibacterial antifouling coating provided in Example 8. 2 O 3 Base.
[0071] Depend on Figure 4 It can be seen that: Al 2 O 3 The water contact angles of PVC and PVC decreased from 89.62° and 78.08° to 63.54° and 60.49° respectively after being coated with AMPE coating, both showing good coating effects, which shows that AMPE coating is applicable on different substrates.
[0072] The above experimental results show that the present invention screened out various reaction raw material compositions through a large number of experiments and synthesized a rutin-modified prepolymer, which not only has a high antibacterial rate (≥97%), but also exhibits good hardness, flexibility, adhesion and anti-bacterial adhesion, and achieved good technical effects.
[0073] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing an erythrosine-modified polymer, characterized in that: The following steps are involved: S10. Mixing the erythrosine derivative, the amino bromide and the solvent, heating the mixture to cause an amination reaction to obtain an aminoerythrosine derivative; S20. mixing the first monomer and the second monomer, causing a copolymerization reaction to occur, to obtain a copolymer, wherein the first monomer contains a carboxyl group and a carbon-carbon double bond, and the second monomer contains a double bond and a halogenated alkyl group connected to the double bond; S30. The copolymer is subjected to an elimination reaction to remove the hydrogen halide to obtain a branched copolymer having double bonds; S40. Mixing the aminoerythrosine derivative with the copolymer having double bonds in the side chains, causing an amidation reaction, and obtaining the erythrosine-modified polymer.
2. The method for preparing an erythrosine-based modified polymer as claimed in claim 1, wherein In step S10, the erythrosine derivative includes erythrosine B sodium salt; and / or, Aminobromides include 3-bromopropylamine hydrobromide; and / or, The solvent includes any one of dimethylformamide and dimethyl sulfoxide.
3. The preparation method of erythrosin-based modified polymer as claimed in claim 1, wherein In step S10, the molar ratio of the erythrosine derivative to the amino bromide is 1:(1-2), wherein the concentration of the erythrosine derivative in the solvent is 0.01-0.1 mol / L.
4. The preparation method of erythrosin-based modified polymer as claimed in claim 1, wherein In step S10, the heating temperature is 70-90° C.; and / or, In step S10, the heating time is 6 to 8 hours.
5. The preparation method of erythrosin-based modified polymer as claimed in claim 1, wherein The first monomer includes acrylic acid, and the second monomer includes 5-bromo-1-pentene.
6. The preparation method of erythrosin-based modified polymer as claimed in claim 5, wherein Step S20 also includes the following steps: The first monomer, the second monomer and the third monomer are mixed and copolymerized to obtain a copolymer, wherein the first monomer contains a carboxyl group and a carbon-carbon double bond, the second monomer contains a carbon-carbon double bond and a halogenated alkyl connected to the double bond; and the third monomer contains a carbon-carbon double bond and a polyethylene glycol group.
7. The preparation method of erythrosin-based modified polymer as claimed in claim 6, wherein The first monomer is acrylic acid, the second monomer is 5-bromo-1-pentene, and the third monomer is polyethylene glycol methacrylate.
8. The preparation method of erythrosin-based modified polymer as claimed in claim 6, wherein In step S20 , the mass ratio of the first monomer, the second monomer, and the third monomer is 1:(5-9):(0-4).
9. An erythrosine-modified polymer, characterized in that The erythrosin-modified polymer is prepared according to the preparation method of any one of claims 1 to 8.
10. A coating, characterized in that: It comprises an erythrin-modified polymer and a free radical photoinitiator, wherein the erythrin-modified polymer is the erythrin-modified polymer as claimed in claim 9.
Citation Information
Patent Citations
Preparation method of mud resisting and slump retaining type phosphate group containing polycarboxylate superplasticizer
CN106008853A
Core-shell type molecularly imprinted polymer capable of recognizing erythrosine and preparation method
CN107266627A