Phosphorus-containing flame-retardant toughening agent as well as preparation method and application thereof

By using phosphorus-containing acrylate flame retardant with acrylate, initiator and crosslinking agent in polycarbonate materials, the problem of difficult to take into account both the flame retardant and impact resistance of polymer materials is achieved, and polycarbonate is realized The excellent flame retardant and impact resistance of the ester materials meet the safety standards of the automobile industry.

CN118978638APending Publication Date: 2024-11-19WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163943.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In automotive applications, existing polymer materials are difficult to take into account both flame retardant and impact resistance. The addition of toughener often reduces flame retardant efficiency and cannot meet stricter safety standards.

Method used

The phosphorus-containing acrylate flame retardant is used to combine with acrylate, initiator and crosslinking agent to form a phosphorus-containing flame retardant toughening agent with excellent flame retardant and toughening properties, and is used in polycarbonate materials to improve resistance. Flame and impact resistance.

Benefits of technology

Composite materials with an ultimate oxygen index of ≥28.8%, vertical combustion level above V-1 and impact strength ≥67.8kJ·m-2 were obtained to meet the safety needs of the automobile industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007281810000021
    Figure BDA0005007281810000021
  • Figure BDA0005007281810000041
    Figure BDA0005007281810000041
  • Figure BDA0005007281810000042
    Figure BDA0005007281810000042
Patent Text Reader

Abstract

The invention relates to a phosphorus-containing flame-retardant toughening agent as well as a preparation method and application thereof. The phosphorus-containing flame-retardant toughening agent is prepared from the following raw materials: a phosphorus-containing acrylate flame retardant with a specific structure, first acrylate, an initiator and a cross-linking agent. The phosphorus-containing flame-retardant toughening agent provided by the invention comprises the phosphorus-containing acrylate flame retardant which can simultaneously realize flame retardance and toughening and has a specific structure, the phosphorus-containing acrylate flame retardant is compounded with the acrylate, the initiator and the cross-linking agent, so that the flame retardance and impact resistance are further improved, the phosphorus-containing flame-retardant toughening agent is applied to a polycarbonate material, and the flame retardance and impact resistance of the polycarbonate material are improved. The composite material with excellent flame retardance and toughness can be obtained, and the application requirements in the fields of automobile industry and the like can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material synthesis, and in particular to a phosphorus-containing flame retardant toughening agent and a preparation method and application thereof. Background Art

[0002] With the rapid popularization of new energy vehicles, in order to pursue higher energy efficiency and endurance, polymer materials as a lightweight material, such as polycarbonate (PC), can reduce the overall weight of the vehicle and increase the electric range. However, generally speaking, polymer materials themselves have poor flame retardant properties, and due to the presence of batteries and electrical systems, cars have a greater risk of spontaneous combustion, which increases the demand for the flame retardant properties of the materials themselves to meet more stringent safety standards. For example, CN105462208A provides a flame retardant reinforced polycarbonate material, which is composed of the following weight ratio raw materials: polycarbonate raw material: 50-70; glass fiber: 20-40; antioxidant: 1.0; dispersing lubricant: 1.0; titanate coupling agent: 1.0; antimony trioxide: 4.0-6.0; dispersant: 4.0-6.0, which does not affect the mechanical properties of the material and improves the flame retardancy of PC.

[0003] At the same time, when polymer materials are applied to the automotive field, the materials are required to have higher impact strength, absorb more energy in the event of a collision, and protect the safety of the vehicle and passengers. CN102532855A provides a polycarbonate injection molding grade toughening agent with good toughening effect and low cost, a preparation method thereof, and a toughened polycarbonate with the toughening agent added. The composition of the polycarbonate injection molding grade toughening agent is expressed by weight as follows: 30-50 acrylate polymer; 50-70 acrylate grafted styrene elastomer; 0.1-0.3 antioxidant. The composition of the toughened polycarbonate is expressed by weight as follows: 5-10 polycarbonate toughening agent, 90-95 polycarbonate. The preparation method of the polycarbonate injection molding grade toughening agent is as follows: (1) adding an acrylic polymer, an acrylic grafted styrene elastomer, and an antioxidant into a mixer and mixing them until they are uniform; (2) feeding the mixed materials into a feeding hopper of a twin-screw extruder, mixing and plasticizing them through the twin-screw extruder, and then extruding them; (3) forming the extruded materials into granules; and (4) drying the granules.

[0004] Although flame retardants and toughening agents can be added to polymer materials to improve their flame retardancy and toughness, since most toughening agents are also flammable materials, adding toughening agents often reduces the flame retardant efficiency of flame retardants, thus failing to achieve the desired effect. Therefore, the art urgently needs to develop a high-efficiency toughening agent with flame retardant properties to take into account the impact resistance and flame retardant properties of the material itself. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a phosphorus-containing flame retardant and toughening agent, a preparation method and application thereof, wherein the phosphorus-containing flame retardant and toughening agent includes a phosphorus-containing acrylate flame retardant with a specific structure having excellent flame retardancy and toughening properties, and further compounding the phosphorus-containing acrylate with acrylate, initiator and crosslinking agent to optimize the flame retardancy and impact resistance of the material. The phosphorus-containing flame retardant and toughening agent is applied to PC materials to obtain a composite material with both excellent flame retardancy and toughness, meeting the application needs in the automotive industry and other fields.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a phosphorus-containing flame retardant and toughening agent, wherein the raw materials for preparing the phosphorus-containing flame retardant and toughening agent include a combination of a phosphorus-containing acrylate flame retardant, a first acrylate, an initiator and a crosslinking agent;

[0008] The phosphorus-containing acrylate flame retardant includes a compound having a structure as shown in Formula I:

[0009]

[0010] Wherein, said R1 is selected from hydrogen or methyl;

[0011] The R2 and R3 are each independently selected from a straight or branched chain alkyl group of C1-C5 (eg, C2, C3, C4).

[0012] The phosphorus-containing flame retardant toughening agent provided by the present invention includes a combination of a phosphorus-containing acrylate flame retardant, a first acrylate, an initiator and a cross-linking agent. By compounding a phosphorus-containing acrylate flame retardant with other components using a specific structure, a phosphorus-containing flame retardant toughening agent with excellent flame retardancy and impact resistance is obtained. The phosphorus-containing acrylate flame retardant used in the present invention contains a phosphonate structure and an acrylate structure, so that it has both the flame retardancy of a general phosphorus-containing flame retardant and a toughening effect. Compared with general phosphate compounds, the phosphorus-containing acrylate flame retardant used in the present invention has a controllable reaction when cross-linked with other components, and the chain segments of other components are not easily inserted into the phosphonate structure, so the grafting effect is better, and the obtained phosphorus-containing flame retardant toughening agent has more excellent application performance.

[0013] Preferably, in parts by weight, the phosphorus-containing flame retardant toughening agent includes 150-200 parts of a phosphorus-containing acrylate flame retardant, 200-300 parts of a first acrylate, 1-5 parts of an initiator, and 1-10 parts of a cross-linking agent.

[0014] The weight proportion of the phosphorus-containing acrylate flame retardant is 150-200 parts, for example, 155 parts, 160 parts, 165 parts, 170 parts, 175 parts, 180 parts, 185 parts, 190 parts or 195 parts.

[0015] The weight proportion of the first acrylate is 200-300 parts, for example, 210 parts, 220 parts, 230 parts, 240 parts, 250 parts, 260 parts, 270 parts, 280 parts or 290 parts.

[0016] The weight portion of the initiator is 1-5 parts, for example, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts or 4.5 parts.

[0017] The weight portion of the cross-linking agent is 1-10 parts, for example, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 9.5 parts.

[0018] The “parts” and “parts by weight” involved in the present invention are all calculated based on solid content and do not include solvents, dispersants, etc.

[0019] The phosphorus-containing acrylate flame retardant includes a compound having a structure shown in Formula II and / or Formula III:

[0020]

[0021] The present invention preferably uses compounds of the structure shown in Formula II and / or Formula III, which can make the molecular weight of the product obtained by the subsequent polymerization reaction more controllable, the proportion of phosphorus element higher, and the flame retardant effect better.

[0022] Preferably, the phosphorus-containing acrylate flame retardant is prepared by the following method: a phosphonate is reacted with a second acrylate to obtain the phosphorus-containing acrylate flame retardant.

[0023] Preferably, the phosphonate has a structure as shown in Formula IV:

[0024]

[0025] Wherein, R4 is selected from a straight chain or branched chain alkyl group of C1-C5 (for example, C2, C3, C4), and the selection of R2 and R3 is the same as that of Formula I.

[0026] Preferably, the phosphonate comprises dimethyl methylphosphonate.

[0027] Preferably, the second acrylate includes any one of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate or butyl acrylate, or a combination of at least two thereof.

[0028] Preferably, the reaction is carried out in the presence of a catalyst.

[0029] Preferably, the catalyst comprises an ionic liquid catalyst.

[0030] Preferably, the ionic liquid catalyst comprises 1-butyl-3-methylimidazolium tetrafluoroborate and / or 1-butyl-3-methylimidazolium hexafluorophosphate.

[0031] Preferably, the molar ratio of the phosphonate to the second acrylate is (1-1.5):1, for example, 1.1:1, 1.2:1, 1.3:1, 1.4:1, etc.

[0032] Preferably, based on 100 parts of the total mass of the phosphonate and the second acrylate, the amount of the catalyst is 0.5-2 parts, for example, 0.6 parts, 0.8 parts, 1 parts, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, etc.

[0033] Preferably, the reaction temperature is 70-80°C, for example, it can be 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, etc.

[0034] Preferably, the reaction time is 6-8 h, for example, it can be 6.2 h, 6.5 h, 6.8 h, 7 h, 7.2 h, 7.5 h, 7.8 h, etc.

[0035] Preferably, the reaction is carried out under stirring.

[0036] Preferably, the stirring speed is 200-300 rpm, for example, 220 rpm, 240 rpm, 260 rpm, 280 rpm, etc.

[0037] Preferably, the first acrylic acid ester includes any one of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate or butyl acrylate, or a combination of at least two thereof.

[0038] Preferably, the initiator comprises a persulfate.

[0039] Preferably, the initiator includes any one of potassium persulfate, sodium persulfate or ammonium persulfate, or a combination of at least two thereof.

[0040] Preferably, the crosslinking agent comprises an acrylate crosslinking agent.

[0041] Preferably, the crosslinking agent includes any one of 1,4-butylene glycol diacrylate, ethylene glycol dimethacrylate or 1,2-butylene glycol dimethacrylate, or a combination of at least two thereof.

[0042] Preferably, the raw materials for preparing the phosphorus-containing flame retardant and toughening agent further include 1-10 parts of emulsifier, for example, 2 parts, 3 parts, 5 parts, 7 parts or 9 parts, etc., by weight.

[0043] Preferably, the emulsifier comprises an anionic emulsifier.

[0044] Preferably, the emulsifier includes any one of sodium dodecyl sulfate, sodium dodecyl sulfonate or sodium dodecylbenzene sulfonate, or a combination of at least two thereof.

[0045] In a second aspect, the present invention provides a method for preparing the phosphorus-containing flame retardant toughening agent as described in the first aspect, the preparation method comprising the following steps:

[0046] The phosphorus-containing acrylate flame retardant, the first acrylate, the initiator, the crosslinking agent and the optional emulsifier are mixed and reacted to obtain the phosphorus-containing flame retardant toughening agent.

[0047] Preferably, the preparation method comprises the following steps:

[0048] (1) mixing a portion of the first acrylate, a portion of the emulsifier, a portion of the cross-linking agent and a solvent for pre-emulsification to obtain a first pre-emulsion;

[0049] (2) taking part of the first pre-emulsion obtained in step (1), heating and stirring, mixing with part of the initiator and the solvent to initiate polymerization, and after blue light appears, adding the remaining first pre-emulsion to obtain an acrylate core emulsion;

[0050] (3) pre-emulsifying the phosphorus-containing acrylate flame retardant with the remaining first acrylate, the remaining emulsifier, the remaining cross-linking agent, and the solvent to obtain a second pre-emulsification, mixing the second pre-emulsion with the acrylate core emulsion obtained in step (2), adding the remaining initiator to react, and obtaining a phosphorus-containing flame retardant toughening agent emulsion;

[0051] (4) adding a calcium chloride aqueous solution to the phosphorus-containing flame retardant and toughening agent emulsion obtained in step (3), heating and stirring to break the emulsion, and stopping the reaction after obvious sanding is observed in the emulsion to obtain the phosphorus-containing flame retardant and toughening agent.

[0052] In the present invention, the sand production refers to the appearance of fine granular precipitation in the emulsion.

[0053] Preferably, in parts by weight, the first acrylate in step (1) is 100-200 parts (for example, 110 parts, 130 parts, 150 parts, 170 parts, 190 parts, etc.), the emulsifier is 0.5-5 parts (for example, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, etc.), the cross-linking agent is 0.5-5 parts (for example, 0.8 parts, 1 part, 2 parts, 3 parts, 4 parts, etc.), and the solvent is 150-300 parts (for example, 160 parts, 180 parts, 200 parts, 220 parts, 240 parts, 260 parts, 280 parts, etc.).

[0054] Preferably, the solvent comprises water.

[0055] Preferably, the mixing method in step (1) is stirring.

[0056] Preferably, the first pre-emulsion obtained from the portion of step (1) in step (2) accounts for 10-20% of the total mass of the first pre-emulsion, for example, it can be 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, etc.

[0057] Preferably, the heating temperature in step (2) is 70-90°C, for example, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, etc.

[0058] Preferably, the stirring speed in step (2) is 150-200 rpm, for example, 160 rpm, 170 rpm, 180 rpm, 190 rpm, etc.

[0059] Preferably, the weight proportion of the part of the initiator in step (2) is 0.5-2.5 parts (for example, it can be 0.6 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, etc.), and the weight proportion of the solvent is 100-300 parts (for example, it can be 120 parts, 150 parts, 180 parts, 200 parts, 220 parts, 250 parts, 280 parts, etc.).

[0060] Preferably, the remaining first pre-emulsion in step (2) is 80-90% of the total mass of the first pre-emulsion, for example, it can be 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, etc.

[0061] Preferably, the method of adding the remaining first pre-emulsion in step (2) comprises dropwise addition.

[0062] Preferably, after adding the remaining first pre-emulsion in step (2), the reaction is continued for 2-3 hours, for example, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, etc.

[0063] Preferably, in parts by weight, the phosphorus-containing acrylate flame retardant in step (3) is 150-200 parts (for example, 155 parts, 160 parts, 165 parts, 170 parts, 175 parts, 180 parts, 185 parts, 190 parts, 195 parts, etc.), the remaining first acrylate is 100-200 parts (for example, 110 parts, 130 parts, 150 parts, 170 parts, 190 parts, etc.), and the remaining emulsifier is 0.5-5 parts (for example, 1 part, 1.5 parts, 2 parts). , 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, etc.), the remaining cross-linking agent is 0.5-5 parts (for example, it can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, etc.), the solvent is 300-350 parts (for example, it can be 310 parts, 320 parts, 330 parts, 340 parts, etc.), and the remaining initiator is 0.5-2.5 parts (for example, it can be 0.6 parts, 0.8 parts, 1 part, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, etc.).

[0064] Preferably, in step (3), the second pre-emulsion and the acrylate core emulsion are mixed by dropwise addition.

[0065] Preferably, the method of adding the initiator in step (3) includes dropwise addition.

[0066] Preferably, the reaction temperature in step (3) is 70-90°C, for example, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, etc.

[0067] Preferably, the reaction time in step (3) is 2-4 h, for example, it can be 2.2 h, 2.5 h, 2.8 h, 3 h, 3.2 h, 3.5 h, 3.8 h, etc.

[0068] Preferably, the reaction in step (3) is carried out under stirring.

[0069] Preferably, the stirring speed is 150-200 rpm, for example, 160 rpm, 170 rpm, 180 rpm, 190 rpm, etc.

[0070] Preferably, the mass concentration of the calcium chloride aqueous solution in step (4) is 5-10%, for example, 5.5%, 6%, 7%, 8%, 9%, etc.

[0071] Preferably, the speed of adding the calcium chloride aqueous solution in step (4) is 1-30 mL / min, for example, it can be 2 mL / min, 5 mL / min, 8 mL / min, 10 mL / min, 12 mL / min, 15 mL / min, 20 mL / min, 25 mL / min, etc.

[0072] Preferably, the heating temperature in step (4) is 50-70°C, for example, 52°C, 55°C, 58°C, 60°C, 62°C, 65°C, 68°C, etc.

[0073] Preferably, the stirring speed in step (4) is 150-200 rpm, for example, 160 rpm, 170 rpm, 180 rpm, 190 rpm, etc.

[0074] Preferably, after stopping the reaction in step (4), filtering and drying are performed.

[0075] Preferably, the drying is carried out in a forced air drying oven.

[0076] Preferably, the drying temperature is 60-75°C, for example, 62°C, 65°C, 68°C, 70°C, 72°C, etc.

[0077] Preferably, the drying time is 36-48 hours, for example, it can be 38 hours, 40 hours, 42 hours, 44 hours, 46 hours, etc.

[0078] In a third aspect, the present invention provides a flame retardant polycarbonate, comprising polycarbonate and the phosphorus-containing flame retardant toughening agent as described in the first aspect.

[0079] Preferably, the flame retardant polycarbonate comprises 78-93 parts of polycarbonate and 5-20 parts of phosphorus-containing flame retardant toughening agent, in parts by weight.

[0080] The weight proportion of the polycarbonate is 78-95 parts, for example, 80 parts, 82 parts, 85 parts, 88 parts, 90 parts, 92 parts, etc.

[0081] The weight portion of the phosphorus-containing flame retardant toughening agent is 5-20 parts, for example, 6 parts, 8 parts, 10 parts, 12 parts, 15 parts, 18 parts, etc.

[0082] Preferably, the flame retardant polycarbonate further comprises 0.5-1 part of lubricant, for example, 0.55 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, etc., by weight.

[0083] Preferably, the lubricant comprises sodium stearate.

[0084] Preferably, the flame retardant polycarbonate further comprises 0.5-1 part of a composite antioxidant, for example, 0.55 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, etc., by weight.

[0085] Preferably, the composite antioxidant comprises a combination of at least two of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and triester (2,4-di-tert-butylphenyl)phosphite.

[0086] Specific examples of the composite antioxidant include Antioxidant 1010, Antioxidant 1076, Antioxidant 168, and the like.

[0087] Preferably, the flame retardant polycarbonate is prepared by the following method:

[0088] The flame retardant polycarbonate is obtained by mixing polycarbonate, a phosphorus-containing flame retardant toughening agent, an optional lubricant and an optional composite antioxidant, and extruding the mixture.

[0089] Preferably, the extrusion is carried out in a twin-screw extruder.

[0090] Preferably, the extrusion temperature is 80-310°C, for example, it can be 90°C, 100°C, 120°C, 150°C, 180°C, 200°C, 220°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C, etc.

[0091] In a fourth aspect, the present invention provides a use of the phosphorus-containing flame retardant toughening agent as described in the first aspect or the flame retardant polycarbonate as described in the third aspect in automotive materials.

[0092] Compared with the prior art, the present invention has at least the following beneficial effects:

[0093] The phosphorus-containing flame retardant toughening agent provided by the present invention comprises a combination of a phosphorus-containing acrylate flame retardant, a first acrylate, an initiator and a crosslinking agent, wherein the phosphorus-containing acrylate flame retardant structure comprises a phosphonate structure and an acrylate structure, so that it has both flame retardant properties and a toughening effect. By compounding the phosphorus-containing acrylate flame retardant with a specific structure and other components, a phosphorus-containing flame retardant toughening agent with excellent flame retardant and impact resistance is obtained. The phosphorus-containing flame retardant toughening agent is applied to a polycarbonate material, and the obtained flame retardant polycarbonate has a limiting oxygen index of ≥28.8%, a vertical combustion level of above V-1, and an impact strength of ≥67.8 kJ·m -2 . DETAILED DESCRIPTION

[0094] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0095] In the following specific implementation of the present invention, the materials involved are as follows:

[0096] Polycarbonate:

[0097] Wanhua Chemical, WANBLEND CA1450

[0098] Antioxidants:

[0099] BASF, IRGAFOS168, IRGANOX 1076

[0100] Preparation Example 1

[0101] A phosphorus-containing acrylate flame retardant, wherein the phosphorus-containing acrylate flame retardant has a structure as shown in Formula III:

[0102]

[0103] The phosphorus-containing acrylate flame retardant is prepared by the following method:

[0104] Weigh 186g of dimethyl methylphosphonate, 100g of methyl methacrylate and 3g of ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate, put them into a three-necked flask equipped with a condenser and a thermometer, and react at 80°C for 6h to obtain a phosphorus-containing acrylate flame retardant represented by formula III. 1 H-NMR detection: δ = 1.43 (d, 3H, P-CH3), δ = 2.01 (s, 3H, C-CH3), δ = 3.66 (d, 3H, PO-CH3), δ = 6.30 (d, 2H, C = CH2).

[0105] Preparation Example 2

[0106] A phosphorus-containing acrylate flame retardant, the phosphorus-containing acrylate flame retardant has a structure as shown in formula III, and the phosphorus-containing acrylate flame retardant is prepared by the following method:

[0107] Weigh 186 g of dimethyl methylphosphonate and 100 g of methyl methacrylate, put them into a three-necked flask equipped with a condenser and a thermometer, and react at 80° C. for 12 h to obtain a phosphorus-containing acrylate flame retardant represented by formula III.

[0108] By comparing the phosphorus-containing acrylate flame retardants obtained in Preparation Example 1 and Preparation Example 2, it can be found that the use of ionic liquid as a catalyst in the present invention can effectively shorten the reaction time. At the same time, the ionic liquid used contains flame retardant elements such as fluorine and boron, which has a certain flame retardant effect and does not need to be specially removed in subsequent reactions.

[0109] Example 1

[0110] A phosphorus-containing flame retardant toughening agent, comprising 178 parts of the phosphorus-containing acrylate flame retardant obtained in Preparation Example 1, 192 parts of butyl acrylate, 50 parts of methyl methacrylate, 4 parts of an emulsifier sodium dodecyl sulfonate, 2 parts of an initiator potassium persulfate, and 1 part of a cross-linking agent 1,2-butanediol dimethacrylate;

[0111] The phosphorus-containing flame retardant toughening agent is prepared by the following method:

[0112] 192 parts of butyl acrylate, 2 parts of emulsifier, 0.5 parts of crosslinking agent and 300 parts of deionized water were added into a container and pre-emulsified for 30 minutes at a stirring speed of 500 rpm to obtain a first pre-emulsion.

[0113] Take 20wt% of the first pre-emulsion, add 1 part of initiator and 200 parts of deionized water, heat to 80°C in a constant temperature water bath to initiate polymerization, and maintain a rotation speed of 150rpm. After the blue light appears, start to add the remaining first pre-emulsion at a dropping speed of 5mL / min. After the addition is completed, continue stirring the reaction for 2h to obtain an acrylate core emulsion.

[0114] 178 parts of phosphorus-containing acrylate flame retardant, 50 parts of methyl methacrylate, 2 parts of emulsifier, 0.5 parts of crosslinking agent and 300 parts of deionized water were added into a container and pre-emulsified at a stirring speed of 500 rpm for 30 minutes to obtain a second pre-emulsion.

[0115] Heat the acrylate core emulsion to 80°C in a constant temperature water bath and maintain the rotation speed at 150rpm. Slowly add the second pre-emulsion to the acrylate core emulsion at a dropping speed of 5mL / min. 10 minutes after the addition, add 1 part of the initiator. Continue stirring the reaction for 2h to obtain a phosphorus-containing flame retardant toughening agent emulsion.

[0116] The phosphorus-containing flame retardant and toughening agent emulsion was heated to 70° C. in a constant temperature water bath and the rotation speed was maintained at 150 rpm. A 5% mass concentration of calcium chloride aqueous solution was added dropwise to the phosphorus-containing flame retardant and toughening agent emulsion for demulsification. The dropping speed was 15 mL / min. After obvious sand production was observed, the dropping was stopped, and the heating and stirring were turned off. The phosphorus-containing flame retardant and toughening agent was washed with deionized water, filtered, and dried to obtain a powdered phosphorus-containing flame retardant and toughening agent.

[0117] Example 2

[0118] A phosphorus-containing flame retardant toughening agent, the phosphorus-containing flame retardant toughening agent comprising 190 parts of the phosphorus-containing acrylate flame retardant obtained in Preparation Example 2, 280 parts of ethyl methacrylate, 7 parts of an emulsifier, 4 parts of an initiator, sodium persulfate, and 8 parts of a crosslinking agent, 1,4-butylene glycol diacrylate;

[0119] The phosphorus-containing flame retardant toughening agent is prepared by the following method:

[0120] 210 parts of ethyl methacrylate, 3.5 parts of emulsifier, 4 parts of crosslinking agent and 250 parts of deionized water were added into a container and pre-emulsified at a stirring speed of 500 rpm for 30 minutes to obtain a first pre-emulsion.

[0121] Take 15wt% of the first pre-emulsion, add 2 parts of initiator and 230 parts of deionized water, heat to 80°C in a constant temperature water bath to initiate polymerization, and maintain a rotation speed of 150rpm. After the blue light appears, start to add the remaining first pre-emulsion at a dropping speed of 5mL / min. After the addition is completed, continue stirring the reaction for 2h to obtain an acrylate core emulsion.

[0122] 190 parts of phosphorus-containing acrylate flame retardant, 70 parts of ethyl methacrylate, 3.5 parts of emulsifier, 4 parts of crosslinking agent and 330 parts of deionized water were added into a container and pre-emulsified for 30 minutes at a stirring speed of 500 rpm to obtain a second pre-emulsion.

[0123] Heat the acrylate core emulsion to 80°C in a constant temperature water bath and maintain the rotation speed at 150rpm. Slowly add the second pre-emulsion to the acrylate core emulsion at a dropping speed of 5mL / min. 10 minutes after the addition, add 2 parts of initiator and continue stirring the reaction for 2h to obtain a phosphorus-containing flame retardant toughening agent emulsion.

[0124] The phosphorus-containing flame retardant and toughening agent emulsion was heated to 70° C. in a constant temperature water bath and the rotation speed was maintained at 150 rpm. An 8% mass concentration of calcium chloride aqueous solution was added dropwise to the phosphorus-containing flame retardant and toughening agent emulsion for demulsification. The dropping speed was 15 mL / min. After obvious sand production was observed, the dropping was stopped, and the heating and stirring were turned off. The phosphorus-containing flame retardant and toughening agent was washed with deionized water, filtered, and dried to obtain a powdered phosphorus-containing flame retardant and toughening agent.

[0125] Example 3

[0126] A phosphorus-containing flame retardant toughening agent, comprising 155 parts of the phosphorus-containing acrylate flame retardant obtained in Preparation Example 1, 150 parts of butyl methacrylate, 60 parts of methyl acrylate, 2 parts of an emulsifier, 2 parts of an emulsifier, 1 part of an initiator, ammonium persulfate, and 2 parts of a cross-linking agent, ethylene glycol dimethacrylate;

[0127] The phosphorus-containing flame retardant toughening agent is prepared by the following method:

[0128] 150 parts of butyl methacrylate, 1 part of emulsifier, 1 part of crosslinking agent and 160 parts of deionized water were added into a container and pre-emulsified for 30 minutes at a stirring speed of 500 rpm to obtain a first pre-emulsion.

[0129] Take 12wt% of the first pre-emulsion, add 0.5 parts of initiator and 120 parts of deionized water, heat to 80°C in a constant temperature water bath to initiate polymerization, and maintain the rotation speed at 180rpm. After the blue light appears, start to add the remaining first pre-emulsion at a dropping speed of 5mL / min. After the addition is completed, continue stirring the reaction for 2.5h to obtain an acrylate core emulsion.

[0130] 190 parts of phosphorus-containing acrylate flame retardant, 60 parts of methyl acrylate, 1 part of emulsifier, 1 part of crosslinking agent and 310 parts of deionized water were added into a container and pre-emulsified for 30 minutes at a stirring speed of 500 rpm to obtain a second pre-emulsion.

[0131] Heat the acrylate core emulsion to 80°C in a constant temperature water bath and maintain the rotation speed at 150rpm. Slowly add the second pre-emulsion to the acrylate core emulsion at a dropping speed of 5mL / min. 10 minutes after the addition, add 0.5 parts of initiator, continue stirring and reacting for 3h to obtain a phosphorus-containing flame retardant toughening agent emulsion.

[0132] The phosphorus-containing flame retardant and toughening agent emulsion was heated to 65° C. in a constant temperature water bath and the rotation speed was maintained at 150 rpm. A 6% mass concentration of calcium chloride aqueous solution was added dropwise to the phosphorus-containing flame retardant and toughening agent emulsion for demulsification. The dropping speed was 15 mL / min. After obvious sand production was observed, the dropping was stopped, and the heating and stirring were turned off. The phosphorus-containing flame retardant and toughening agent was washed with deionized water, filtered, and dried to obtain a powdered phosphorus-containing flame retardant and toughening agent.

[0133] Example 4

[0134] A phosphorus-containing flame retardant and toughening agent, comprising 89 parts of the phosphorus-containing acrylate flame retardant obtained in Preparation Example 1, 192 parts of butyl acrylate, 100 parts of methyl methacrylate, 4 parts of emulsifier sodium dodecyl sulfate, 2 parts of initiator potassium persulfate, and 1 part of cross-linking agent 1,2-butanediol dimethacrylate.

[0135] The phosphorus-containing flame retardant toughening agent is prepared by the following method:

[0136] 192 parts of butyl acrylate, 2 parts of emulsifier, 0.5 parts of crosslinking agent and 300 parts of deionized water were added into a container and pre-emulsified for 30 minutes at a stirring speed of 500 rpm to obtain a first pre-emulsion.

[0137] Take 20wt% of the first pre-emulsion, add 1 part of initiator and 200 parts of deionized water, heat to 80°C in a constant temperature water bath to initiate polymerization, and maintain a rotation speed of 150rpm. After the blue light appears, start to add the remaining first pre-emulsion at a dropping speed of 5mL / min. After the addition is completed, continue stirring the reaction for 2h to obtain an acrylate core emulsion.

[0138] 89 parts of phosphorus-containing acrylate flame retardant, 100 parts of methyl methacrylate, 2 parts of emulsifier, 0.5 parts of crosslinking agent and 300 parts of deionized water were added into a container and pre-emulsified at a stirring speed of 500 rpm for 30 minutes to obtain a second pre-emulsion.

[0139] Heat the acrylate core emulsion to 80°C in a constant temperature water bath and maintain the rotation speed at 150rpm. Slowly add the second pre-emulsion to the acrylate core emulsion at a dropping speed of 5mL / min. 10 minutes after the addition, add 1 part of the initiator. Continue stirring the reaction for 2h to obtain a phosphorus-containing flame retardant toughening agent emulsion.

[0140] The phosphorus-containing flame retardant and toughening agent emulsion was heated to 70° C. in a constant temperature water bath and the rotation speed was maintained at 150 rpm. A 5% mass concentration of calcium chloride aqueous solution was added dropwise to the phosphorus-containing flame retardant and toughening agent emulsion for demulsification. The dropping speed was 15 mL / min. After obvious sand production was observed, the dropping was stopped, and the heating and stirring were turned off. The phosphorus-containing flame retardant and toughening agent was washed with deionized water, filtered, and dried to obtain a powdered phosphorus-containing flame retardant and toughening agent.

[0141] Comparative Example 1

[0142] A flame retardant toughening agent. Compared with Example 1, this comparative example does not add a phosphorus-containing acrylate flame retardant. The flame retardant toughening agent includes 192 parts of butyl acrylate, 150 parts of methyl methacrylate, 3 parts of an emulsifier sodium dodecyl sulfonate, 2 parts of an initiator potassium persulfate, and 1 part of a cross-linking agent 1,2-butanediol dimethacrylate.

[0143] The flame retardant toughening agent is prepared by the following method:

[0144] 192 parts of butyl acrylate, 2 parts of emulsifier, 0.5 parts of crosslinking agent and 300 parts of deionized water were added into a container and pre-emulsified for 30 minutes at a stirring speed of 500 rpm to obtain a first pre-emulsion.

[0145] Take 20wt% of the first pre-emulsion, add 1 part of initiator and 200 parts of deionized water, heat to 80°C in a constant temperature water bath to initiate polymerization, and maintain a rotation speed of 150rpm. After the blue light appears, start to add the remaining first pre-emulsion at a dropping speed of 5mL / min. After the addition is completed, continue stirring the reaction for 2h to obtain an acrylate core emulsion.

[0146] 150 parts of methyl methacrylate, 1 part of emulsifier, 0.5 parts of crosslinking agent and 300 parts of deionized water were added into a container and pre-emulsified at a stirring speed of 500 rpm for 30 minutes to obtain a second pre-emulsion.

[0147] Heat the acrylate core emulsion to 80°C in a constant temperature water bath and maintain the rotation speed at 150rpm. Slowly add the second pre-emulsion to the acrylate core emulsion at a dropping speed of 5mL / min. 10 minutes after the addition, add 1 part of the initiator and continue stirring the reaction for 2h to obtain the toughening agent emulsion.

[0148] The phosphorus-containing flame retardant and toughening agent emulsion is heated to 70° C. in a constant temperature water bath and the rotation speed is maintained at 150 rpm. A 5% mass concentration of calcium chloride aqueous solution is added dropwise to the toughening agent emulsion for demulsification. The dropping speed is 15 mL / min. After obvious sand production is observed, the dropping is stopped, and the heating and stirring are turned off. The flame retardant and toughening agent is washed with deionized water, filtered, and dried to obtain the powdered flame retardant and toughening agent.

[0149] Comparative Example 2

[0150] A phosphorus-containing flame retardant and toughening agent. Compared with Example 1, no crosslinking agent is added in this comparative example. The phosphorus-containing flame retardant and toughening agent includes 178 parts of the phosphorus-containing acrylate flame retardant obtained in Preparation Example 1, 192 parts of butyl acrylate, 50 parts of methyl methacrylate, 4 parts of emulsifier sodium dodecyl sulfate, and 2 parts of initiator potassium persulfate.

[0151] The phosphorus-containing flame retardant toughening agent is prepared by the following method:

[0152] 192 parts of butyl acrylate, 2 parts of emulsifier and 300 parts of deionized water were added into a container and pre-emulsified for 30 minutes at a stirring speed of 500 rpm to obtain a first pre-emulsion.

[0153] Take 20wt% of the first pre-emulsion, add 1 part of initiator and 200 parts of deionized water, heat to 80°C in a constant temperature water bath to initiate polymerization, and maintain a rotation speed of 150rpm. After the blue light appears, start to add the remaining first pre-emulsion at a dropping speed of 5mL / min. After the addition is completed, continue stirring the reaction for 2h to obtain an acrylate core emulsion.

[0154] 178 parts of phosphorus-containing acrylate flame retardant, 50 parts of methyl methacrylate, 2 parts of emulsifier and 300 parts of deionized water were added into a container and pre-emulsified at a stirring speed of 500 rpm for 30 minutes to obtain a second pre-emulsion.

[0155] Heat the acrylate core emulsion to 80°C in a constant temperature water bath and maintain the rotation speed at 150rpm. Slowly add the second pre-emulsion to the acrylate core emulsion at a dropping speed of 5mL / min. 10 minutes after the addition, add 1 part of the initiator. Continue stirring the reaction for 2h to obtain a phosphorus-containing flame retardant toughening agent emulsion.

[0156] The phosphorus-containing flame retardant and toughening agent emulsion was heated to 70° C. in a constant temperature water bath and the rotation speed was maintained at 150 rpm. A 5% mass concentration of calcium chloride aqueous solution was added dropwise to the phosphorus-containing flame retardant and toughening agent emulsion for demulsification. The dropping speed was 15 mL / min. After obvious sand production was observed, the dropping was stopped, and the heating and stirring were turned off. The phosphorus-containing flame retardant and toughening agent was washed with deionized water, filtered, and dried to obtain a powdered phosphorus-containing flame retardant and toughening agent.

[0157] Application Example 1-4, Comparative Application Example 1-3

[0158] A flame retardant polycarbonate, the types and amounts of the components are shown in Table 1, and the units of the components in the table are parts by weight;

[0159] The flame retardant polycarbonate is prepared by the following method:

[0160] The components are uniformly mixed according to the ratio, and extruded into granules through a twin-screw extruder. The screw temperatures are 90° C. in zone 1, 240° C. in zone 2, 250° C. in zone 3, 260° C. in zone 4, 270° C. in zone 5, and 280° C. in the die to obtain the flame-retardant polycarbonate.

[0161] Table 1

[0162]

[0163] Perform various performance tests on all application examples and comparative application examples as follows:

[0164] 1) Flame retardant properties:

[0165] The present invention adopts GB / T 2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part II: Room temperature test" to determine the limiting oxygen index (LOI) and GB / T 2408-2008 "Determination of combustion performance of plastics by horizontal and vertical methods" to test the vertical combustion level (UL-94).

[0166] 2) Impact resistance:

[0167] The present invention adopts GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics" to test the notched impact strength.

[0168] The test results are summarized in Table 2.

[0169] Table 2

[0170] The test results show that the present invention uses a phosphorus-containing acrylate flame retardant with a specific structure to compound with acrylate, initiator, and cross-linking agent to obtain a phosphorus-containing flame retardant toughening agent with excellent flame retardancy and impact resistance. When applied to polycarbonate materials, the flame retardancy and impact resistance of the obtained flame-retardant polycarbonate are significantly improved compared with ordinary polycarbonate. By comparing Application Example 1 with Application Example 4, it can be seen that the present invention can achieve better flame retardant effect by further optimizing the amount of phosphorus-containing acrylate flame retardant.

[0171] By comparing Application Example 1 with Comparative Application Examples 1 and 3, it can be seen that the present invention significantly improves the flame retardant properties and impact resistance of polycarbonate by adding a phosphorus-containing flame retardant toughening agent. When the flame retardant is missing, its flame retardant properties are equivalent to those of conventional polycarbonate, and the flame retardant effect cannot be achieved. At the same time, the impact strength is low.

[0172] By comparing Application Example 1 and Comparative Application Example 2, it can be seen that the phosphorus-containing flame retardant toughening agent prepared by compounding with other components by adding a cross-linking agent in the present invention achieves a better toughening effect and improves the flame retardant properties of polycarbonate.

[0173] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A phosphorus-containing flame retardant toughening agent, characterized in that: The raw materials for preparing the phosphorus-containing flame retardant toughening agent include a combination of a phosphorus-containing acrylate flame retardant, a first acrylate, an initiator and a crosslinking agent; The phosphorus-containing acrylate flame retardant includes a compound having a structure as shown in Formula I: Wherein, said R1 is selected from hydrogen or methyl; The R2 and R3 are each independently selected from a C1-C5 straight chain or branched chain alkyl group.

2. The phosphorus-containing flame retardant toughening agent according to claim 1, characterized in that: In parts by weight, the raw materials for preparing the phosphorus-containing flame retardant and toughening agent include 150-200 parts of a phosphorus-containing acrylate flame retardant, 200-300 parts of a first acrylate, 1-5 parts of an initiator, and 1-10 parts of a crosslinking agent.

3. The phosphorus-containing flame retardant toughening agent according to claim 1 or 2, characterized in that: The phosphorus-containing acrylate flame retardant includes a compound having a structure shown in Formula II and / or Formula III: Preferably, the phosphorus-containing acrylate flame retardant is prepared by the following method: a phosphonate is reacted with a second acrylate to obtain the phosphorus-containing acrylate flame retardant; Preferably, the phosphonate has a structure as shown in Formula IV: Wherein, R4 is selected from a C1-C5 straight chain or branched alkyl group, and R2 and R3 are selected in the same manner as in Formula I; Preferably, the phosphonate comprises dimethyl methylphosphonate; Preferably, the second acrylate comprises any one or a combination of at least two of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate or butyl acrylate; Preferably, the reaction is carried out in the presence of a catalyst; Preferably, the catalyst comprises an ionic liquid catalyst; Preferably, the ionic liquid catalyst comprises 1-butyl-3-methylimidazolium tetrafluoroborate and / or 1-butyl-3-methylimidazolium hexafluorophosphate; Preferably, the molar ratio of the phosphonate to the second acrylate is (1-1.5):1; Preferably, the amount of the catalyst is 0.5-2 parts based on 100 parts of the total mass of the phosphonate and the second acrylate; Preferably, the reaction temperature is 70-80°C; Preferably, the reaction time is 6-8h; Preferably, the reaction is carried out under stirring; Preferably, the stirring speed is 200-300 rpm.

4. The phosphorus-containing flame retardant toughening agent according to any one of claims 1 to 3, characterized in that: The first acrylate includes any one or a combination of at least two of methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate or butyl acrylate; Preferably, the initiator comprises a persulfate; Preferably, the initiator comprises any one of potassium persulfate, sodium persulfate or ammonium persulfate, or a combination of at least two thereof; Preferably, the cross-linking agent comprises an acrylate cross-linking agent; Preferably, the crosslinking agent includes any one or a combination of at least two of 1,4-butylene glycol diacrylate, ethylene glycol dimethacrylate or 1,2-butylene glycol dimethacrylate; Preferably, the raw materials for preparing the phosphorus-containing flame retardant and toughening agent further include 1-10 parts of an emulsifier in parts by weight; Preferably, the emulsifier comprises an anionic emulsifier; Preferably, the emulsifier includes any one of sodium dodecyl sulfate, sodium dodecyl sulfonate or sodium dodecylbenzene sulfonate, or a combination of at least two thereof.

5. A method for preparing the phosphorus-containing flame retardant toughening agent according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: The phosphorus-containing acrylate flame retardant, the first acrylate, the initiator, the crosslinking agent and the optional emulsifier are mixed and reacted to obtain the phosphorus-containing flame retardant toughening agent.

6. The preparation method according to claim 5, characterized in that: The preparation method comprises the following steps: (1) mixing a portion of the first acrylate, a portion of the emulsifier, a portion of the cross-linking agent and a solvent for pre-emulsification to obtain a first pre-emulsion; (2) taking part of the first pre-emulsion obtained in step (1), heating and stirring, mixing with part of the initiator and the solvent to initiate polymerization, and after blue light appears, adding the remaining first pre-emulsion to obtain an acrylate core emulsion; (3) pre-emulsifying the phosphorus-containing acrylate flame retardant with the remaining first acrylate, the remaining emulsifier, the remaining cross-linking agent, and the solvent to obtain a second pre-emulsification, mixing the second pre-emulsion with the acrylate core emulsion obtained in step (2), adding the remaining initiator to react, and obtaining a phosphorus-containing flame retardant toughening agent emulsion; (4) adding a calcium chloride aqueous solution to the phosphorus-containing flame retardant and toughening agent emulsion obtained in step (3), heating and stirring to break the emulsion, and stopping the reaction after obvious sanding is observed in the emulsion to obtain the phosphorus-containing flame retardant and toughening agent.

7. The preparation method according to claim 5 or 6, characterized in that: In parts by weight, the first acrylate in step (1) is 100-200 parts, the emulsifier is 0.5-5 parts, the cross-linking agent is 0.5-5 parts, and the solvent is 150-300 parts; Preferably, the solvent comprises water; Preferably, the mixing method in step (1) is stirring; Preferably, the first pre-emulsion obtained from the part of step (1) in step (2) is 10-20% of the total mass of the first pre-emulsion; Preferably, the heating temperature in step (2) is 70-90°C; Preferably, the stirring speed in step (2) is 150-200 rpm; Preferably, the weight portion of the initiator in step (2) is 0.5-2.5 parts, and the weight portion of the solvent is 100-300 parts; Preferably, the remaining first pre-emulsion in step (2) is 80-90% of the total mass of the first pre-emulsion; Preferably, the method of adding the remaining first pre-emulsion in step (2) comprises dropwise addition; Preferably, in step (2), the reaction is continued for 2-3 hours after the remaining first pre-emulsion is added; Preferably, in parts by weight, the phosphorus-containing acrylate flame retardant in step (3) is 150-200 parts, the remaining first acrylate is 100-200 parts, the remaining emulsifier is 0.5-5 parts, the remaining cross-linking agent is 0.5-5 parts, the solvent is 300-350 parts, and the remaining initiator is 0.5-2.5 parts; Preferably, in step (3), the method of mixing the second pre-emulsion with the acrylate core emulsion comprises dropwise addition; Preferably, the method of adding the initiator in step (3) comprises dropwise addition; Preferably, the reaction temperature in step (3) is 70-90°C; Preferably, the reaction time in step (3) is 2-4 hours; Preferably, the reaction in step (3) is carried out under stirring; Preferably, the stirring speed is 150-200 rpm; Preferably, the mass concentration of the calcium chloride aqueous solution in step (4) is 5-10%; Preferably, the calcium chloride aqueous solution is added at a rate of 1-30 mL / min in step (4); Preferably, the heating temperature in step (4) is 50-70°C; Preferably, the stirring speed in step (4) is 150-200 rpm; Preferably, after stopping the reaction in step (4), filtering and drying are performed.

8. A flame retardant polycarbonate, characterized in that: The flame retardant polycarbonate comprises polycarbonate and the phosphorus-containing flame retardant toughening agent according to any one of claims 1 to 4.

9. The flame retardant polycarbonate according to claim 8, characterized in that: In parts by weight, the flame retardant polycarbonate comprises 78-95 parts of polycarbonate and 5-20 parts of a phosphorus-containing flame retardant toughening agent; Preferably, the flame retardant polycarbonate further comprises 0.5-1 part of lubricant by weight; Preferably, the lubricant comprises sodium stearate; Preferably, the flame retardant polycarbonate further comprises 0.5-1 part of a composite antioxidant, by weight; Preferably, the composite antioxidant comprises a combination of at least two of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, n-octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and triester (2,4-di-tert-butylphenyl)phosphite.