Preparation method and application of organic silicon fluid loss agent for well cementation
By using the combination of silicone and nanomaterials on the surface of cement particles, a temperature-resistant and salt-resistant water-reducing agent is formed, which solves the problems of water loss and salt ions in the existing technology under ultra-high temperature environment, and realizes the cement slurry efficient stability and salt resistance.
Patent Information
- Application Number
- CN202411042045.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The existing water-depleting agent fails in ultra-high temperature cementing environments above 200°C and is susceptible to salt ions, which affects the thickening time and rheology performance of the cement slurry.
Using silicone as the main adsorption group, through the condensation mechanism of the surface hydroxyl group of silicon and cement particles, combined with nanomaterials and cationic monomers, the adsorption performance and charge of the polymer are improved, and a temperature-resistant and salt-resistant water-reducing agent is formed. Chemisorption is used to weaken the influence of salt ions.
Effectively reduce the amount of water loss of cement slurry in high-temperature and ultra-high temperature environments, improve suspension stability and salt resistance, temperature resistance to 250℃, and water loss to 25mL, without affecting the performance of the retarder.
Smart Images

Figure BDA0004972630340000061 
Figure BDA0004972630340000071 
Figure BDA0004972630340000081
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of an organosilicon fluid loss reducer for cementing, belonging to the technical field of oilfield chemistry. Background Art
[0002] The development of oil and gas resources is related to the sustainable development of the national economy and society and energy security. With the development of the national economic level, my country's use of oil has continued to increase. At present, with the continuous exploitation of oil and gas, unexploited oil reservoirs have become deeper and denser. For deep oil reservoirs, the high temperature and complex environment make the exploitation process a great obstacle. Cementing is an indispensable and important part of oil and gas exploration and development. Its purpose is to form a strong, dense and durable cement ring between the oil and gas layer and the wellbore to isolate the fluids between different formations and ensure the normal production and safe operation of oil and gas wells. When cementing cement slurry is injected into the wellbore, due to the influence of factors such as formation pressure, temperature, and permeability, water loss will occur, that is, part of the water in the cement slurry is absorbed or squeezed out by the formation. Water loss will lead to adverse consequences such as increased density and viscosity of cement slurry and shortened thickening time, thereby affecting the fluidity and stability of cement slurry in the wellbore, reducing the strength and integrity of the cement ring, and even causing cementing failure. Therefore, controlling the water loss of cement slurry is one of the key technologies to ensure cementing quality.
[0003] Fluid loss reducers can effectively control the amount of cement slurry lost to the formation. However, in deep and ultra-deep well environments, especially after 200°C, conventional linear polymers of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) are prone to hydrolysis and fracture, thereby losing their water loss reduction performance. At the same time, such fluid loss reducers often thicken at low temperatures and dilute at high temperatures in cement slurry systems, which seriously affects the rheological properties and sedimentation stability of high-temperature and ultra-high-temperature cement slurry systems, and thus makes it impossible to guarantee the quality of cementing. Current research has proposed many methods to solve the problem of water loss in cement slurry under high and ultra-high temperature environments.
[0004] Chinese patent document CN 116731262A discloses a constant rheological micro-swelling fluid loss agent, which is obtained by graft copolymerization of sodium methyl propylene sulfonate, acrylamide, acrylic acid, maleic acid and other monomers with allyl polyethylene glycol, ethylene glycol, N-vinyl pyrrolidone and urea. The constant rheological micro-swelling fluid loss agent can achieve constant rheology of cold and hot cement slurry, reduce the influence of temperature on the rheological properties of cement slurry, and control the water loss within 50 ml at 200°C. However, the influence of the fluid loss agent on the thickening performance of cement slurry has not been published. Since a large number of carboxylic acid groups are introduced into the fluid loss agent, the thickening time of cement slurry is easily affected.
[0005] Chinese patent document CN 115404061A discloses a method for preparing a high-temperature and salt-resistant fluid loss reducer composition. Through molecular chain design, conventional disordered polymers are adjusted to block polymers, so that the rigid chains are regularly distributed in the polymer chains, thereby achieving the effects of high-temperature and salt resistance. The rigid chain ends are hydrophilic polymers with better water control ability, which can effectively control the water loss of cement slurry. However, the water loss reduction performance is mainly tested at 120°C, and the performance at other temperatures has not yet been announced. In addition, the fluid loss reducer mainly uses carboxylic acid groups as the main hydrophilic and adsorption groups, which are more likely to affect the performance of the retarder.
[0006] In the article "Preparation and Performance of Fluid Loss Reducer GT-1 for High-Temperature Cementing Slurry" (Zhao Jiansheng et al., Drilling Fluids and Completion Fluids, 2022 / 3), a fluid loss reducer GT-1 for high-temperature cementing slurry was prepared using 2-acrylamido-2-methylpropanesulfonic acid (AMPS), acrylamide (AM), sodium p-styrene sulfonate (SSS), nano-silica, etc. as raw materials. The temperature and salt resistance of the fluid loss reducer were improved by copolymerizing AMPS, AM, and SSS and blending them with nano-silica, which can effectively reduce the water loss of cement slurry under high temperature and high salt conditions. However, there is no specific data on the water loss performance after 200°C, and the presence of AM makes the product prone to hydrolysis and chain breaking in ultra-high temperature environments, thereby affecting the product performance.
[0007] In the article "Preparation and Performance Study of Polymer-based Nano-SiO2 Oil Well Water Loss Agent" (Hao Liangliang et al., Liaoning Chemical Industry, 2023 / 7), a polymer-based nano-SiO2 oil well water loss agent was prepared. The modified nano-silica and hydrophobic associating polymer were connected to improve the temperature and salt resistance and heat resistance of the water loss agent. The water loss was reduced to 48mL at 240°C, and the water loss was less than 80mL when the salinity was within 35%. However, when it was under high salt content, the amount of water loss agent added needed to be greatly increased to maintain its salt resistance.
[0008] Although the prior art represented by the above patents and articles has made breakthroughs in the heat resistance and salt resistance of polymer cementing fluid loss reducers, there are still problems in the application and promotion of ultra-high temperature cementing operations above 200°C. At present, the fluid loss reducers are still mainly carboxylic acid-based fluid loss reducers, and copolymerization with high temperature resistant monomers or grafting with nanoparticles are used as the main means to improve the temperature resistance of the fluid loss reducer, thereby maintaining the heat resistance and salt resistance of the fluid loss reducer. However, since carboxylic acid-based fluid loss reducers are prone to affect the thickening time of cement slurry, and their own performance is easily affected by salt ions, the present invention is aimed at the current use of organic silicon as the main adsorption group to improve the heat resistance and salt resistance of the fluid loss reducer. Summary of the invention
[0009] The invention utilizes the mechanism of condensation of silanol groups in organosilicon and hydroxyl groups on the surface of cement particles in an alkaline environment, introduces organosilicon containing unsaturated double bonds into a polymer as a functional group and a coupling group of a nano material, and can effectively improve the adsorption performance and adsorption strength of the polymer on the surface of cement particles; uses the nano material as the rigid core of the polymer to improve the heat resistance of the polymer; uses a cationic monomer as the charged group of the polymer to increase the charge carried by the cement particles after being adsorbed, thereby improving the dispersion performance of the cement particles; relies on the high heat resistance of the polymer and the strong adsorption effect on the cement particles, so that the fluid loss reducer can effectively reduce the water loss of cement slurry in high temperature and ultra-high temperature environments, and improve the suspension stability of the cement slurry, and the temperature resistance can reach 250°C, and the water loss is reduced to 25mL. At the same time, due to the chemical adsorption method it adopts, it is less susceptible to charge shielding, which can effectively improve the salt resistance of the polymer and ensure the water loss of cement slurry in a high-salt environment. The invented fluid loss reducer does not carry carboxylic acid groups, so it will not produce competitive adsorption with conventional carboxylic acid retarders, thereby reducing the effect of the fluid loss reducer on the retarding time. DETAILED DESCRIPTION OF THE INVENTION
[0011] The technical solution of the present invention is as follows:
[0012] A preparation method of an organosilicon fluid loss additive for cementing:
[0013] A certain amount of nanoparticles, nonionic monomers, cationic monomers and organosilicon are added into a three-necked glass bottle equipped with a stirrer and a condenser, and an appropriate amount of toluene is added as a solvent. The mixture is stirred at a high speed. After all the raw materials are evenly dispersed, nitrogen is introduced for 30 minutes to remove oxygen, and an azo initiator is added. The heating temperature is maintained at 50-70° C. After reacting for 4-10 hours, the product is washed with acetone and ethanol in turn, and then dried and crushed to obtain the desired target product, wherein the monomer concentration is 10-30% of the total mass, the mass ratio of the nanoparticles, nonionic monomers, cationic monomers and organosilicon is 1:(1-16):(1-10):(1-6), and the azo initiator accounts for 0.1-1.5% of the monomer mass.
[0014] According to the present invention, the nonionic monomer is one of N,N-dimethylacrylamide, N,N-dimethylacrylamide and vinyl pyrrolidone, N,N-dimethylacrylamide and styrene, wherein the mass ratio of vinyl pyrrolidone to N,N-dimethylacrylamide is 1:(1.5-3), and the mass ratio of styrene to N,N-dimethylacrylamide is 1:(2-4);
[0015] Preferably, the cationic monomer is one of dodecyl dimethyl allyl ammonium chloride, tetradecyl dimethyl allyl ammonium chloride, hexadecyl dimethyl allyl ammonium chloride, and octadecyl dimethyl allyl ammonium chloride;
[0016] Preferably, the organosilicon is one of γ-methacryloxypropyltrimethoxysilane (KH570), vinyltrimethoxysilane, and allyltrimethylsilane;
[0017] Preferably, the azo initiator is one of azobisisobutylamidine hydrochloride, azobisisobutylonitrile, azobisisobutylimidazoline hydrochloride, and azobisisoheptylonitrile;
[0018] Preferably, the type of nanoparticles is one of nano-silicon dioxide, nano-calcium carbonate, nano-calcium silicate, and nano-bentonite;
[0019] Preferably, the monomer concentration is 15-30% of the total mass, and the mass ratio of the nanoparticles, the nonionic monomer, the cationic monomer and the organosilicon is 1:(1-12):(1-8):(1-3);
[0020] Preferably, the azo initiator accounts for 0.1 to 1.2% of the total weight of the monomers;
[0021] Preferably, the temperature is controlled at 50-65° C. and the polymerization reaction time is 5-8 hours.
[0022] In terms of current general technology, the present invention has the following advantages:
[0023] 1 The present invention utilizes the mechanism of condensation between silanol groups in organosilicon and hydroxyl groups on the surface of cement particles in an alkaline environment, and uses organosilicon containing unsaturated double bonds as a polymerization monomer, and at the same time as an adsorption group and a coupling group of nanoparticles, which can effectively improve the adsorption performance and adsorption strength of the fluid loss reducer on the surface of cement particles; the product uses nanomaterials as the rigid core of the polymer to improve the heat resistance of the polymer, and introduces cationic monomers as charged groups of the polymer to increase the amount of charge carried by the cement particles after being adsorbed, thereby improving the dispersion performance of the cement particles, and further facilitating the formation of a dense filter cake; relying on the heat resistance of the polymer and the strong adsorption effect on cement particles, the fluid loss reducer can effectively reduce the water loss of cement slurry in high temperature and ultra-high temperature environments, and improve the suspension stability of cement slurry.
[0024] 2. The product of the present invention mainly relies on the chemical reaction between silanol and the surface of cement particles, which is a chemical adsorption method. The polymer body is a non-ionic structure and is less susceptible to the charge shielding effect of salt ions. Therefore, it can effectively improve the salt resistance of the polymer and ensure the water loss of cement slurry in a high-salt environment. The invented fluid loss reducer does not carry a carboxylic acid group, making it difficult to produce competitive adsorption with conventional carboxylic acid retarders, thereby reducing the effect of the fluid loss reducer on the retarding time.
[0025] 3. The present invention uses conventional monomers as polymerization raw materials, the molecular weight of the product is controllable, the synthesized fluid loss reducer has no adverse effects on other properties of cement slurry, and the product has good dispersibility and excellent temperature and salt resistance.
[0026] 4. The product prepared by the present invention has good compatibility with the cement slurry system and can effectively reduce the water loss of cement slurry in high temperature, ultra-high temperature and high salt environment. DETAILED DESCRIPTION
[0027] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0028] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources, including:
[0029] In the present invention, N,N-dimethylacrylamide can be purchased commercially, for example, it can be purchased from Jiangsu Bosite Chemical Technology Co., Ltd., industrial grade; vinyl pyrrolidone can be purchased commercially, for example, it can be purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., chemically pure; styrene can be purchased commercially, for example, it can be purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., chemically pure; octadecyl dimethyl allyl ammonium chloride can be purchased commercially, for example, it can be purchased from Guangzhou Shanghe Chemical Technology Co., Ltd., chemically pure; γ-methacryloxypropyl trimethoxysilane can be purchased commercially, for example, it can be purchased from Sinopharm Chemical Reagent Co., Ltd., chemically pure, and dehydrated with molecular sieves for 12 hours; nano-silica can be purchased commercially, for example, it can be purchased from Hubei Huifu Nanomaterials Co., Ltd.
[0030] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0031] Embodiment 1:
[0032] A preparation method of an organosilicon fluid loss additive for cementing:
[0033] 3 parts of nano-silica, 8 parts of N,N-dimethylacrylamide, 4 parts of dodecyldimethylallyl ammonium chloride, 3 parts of γ-methacryloxypropyltrimethoxysilane and 79 parts of toluene were added into a three-necked glass bottle equipped with a nitrogen tube, a stirrer and a condenser, and stirred at high speed. After all the raw materials were evenly dispersed, nitrogen was introduced for 30 minutes, 0.18 parts of azobisisobutyronitrile was added, the heating temperature was maintained at 60°C, and after reacting for 6 hours, the product was washed with acetone and ethanol in turn, and then dried and crushed to obtain the desired target product.
[0034] Embodiment 2:
[0035] As described in Example 1, the difference is that the amount of dodecyl dimethyl allyl ammonium chloride added is 8 parts, and the amount of azobisisobutyronitrile added is 0.24 parts.
[0036] Embodiment 3:
[0037] 1 part of nano-silica, 8 parts of N,N-dimethylacrylamide, 2 parts of dodecyldimethylallyl ammonium chloride, 3 parts of γ-methacryloxypropyltrimethoxysilane and 85 parts of toluene were added into a three-necked glass bottle equipped with a nitrogen tube, a stirrer and a condenser, and stirred at high speed. After all the raw materials were evenly dispersed, nitrogen was introduced for 30 minutes, 0.10 parts of azobisisobutyronitrile were added, the heating temperature was maintained at 60°C, and after reacting for 6 hours, the product was washed with acetone and ethanol in turn, and then dried and crushed to obtain the desired target product.
[0038] Embodiment 4:
[0039] As described in Example 3, except that the amount of γ-methacryloxypropyltrimethoxysilane is 2 parts.
[0040] Embodiment 5:
[0041] 1 part of nano-silica, 10 parts of N,N-dimethylacrylamide, 4 parts of octadecyldimethylallyl ammonium chloride, 3 parts of γ-methacryloxypropyltrimethoxysilane and 81 parts of toluene were added into a three-necked glass bottle equipped with a nitrogen tube, a stirrer and a condenser, and stirred at high speed. After all the raw materials were evenly dispersed, nitrogen was introduced for 30 minutes, 0.10 parts of azobisisobutyronitrile were added, the heating temperature was maintained at 60°C, and after reacting for 6 hours, the product was washed with acetone and ethanol in turn, and then dried and crushed to obtain the desired target product.
[0042] Embodiment 6:
[0043] As described in Example 5, except that the amount of octadecyl dimethyl allyl ammonium chloride added is 2 parts.
[0044] Embodiment 7:
[0045] 1 part of nano-silica, 6 parts of N,N-dimethylacrylamide, 4 parts of vinyl pyrrolidone, 4 parts of octadecyl dimethyl allyl ammonium chloride, 2 parts of vinyl trimethoxy silane and 83 parts of toluene were added into a three-necked glass bottle equipped with a nitrogen tube, a stirrer and a condenser, and stirred at high speed. After all the raw materials were evenly dispersed, nitrogen was introduced for 30 minutes, 0.15 parts of azobisisobutyronitrile were added, the heating temperature was maintained at 65°C, and after reacting for 8 hours, the product was washed with acetone and ethanol in turn, and then dried and crushed to obtain the desired target product.
[0046] Embodiment 8:
[0047] As described in Example 7, except that the amount of vinyl pyrrolidone added was 2 parts.
[0048] Embodiment 9:
[0049] As described in Example 7, except that the amount of vinyltrimethoxysilane added was 3 parts.
[0050] Embodiment 10:
[0051] 0.5 parts of nano-silica, 4 parts of N,N-dimethylacrylamide, 2 parts of styrene, 4 parts of hexadecyldimethylallyl ammonium chloride, 2 parts of vinyltrimethoxysilane and 87.5 parts of toluene were added into a three-necked glass bottle equipped with a nitrogen tube, a stirrer and a condenser, and stirred at high speed. After all the raw materials were evenly dispersed, nitrogen was introduced for 30 minutes, 0.12 parts of azobisisobutyronitrile were added, the heating temperature was maintained at 65°C, and the reaction was continued for 8 hours. After washing with acetone and ethanol in turn, the product was dried and crushed to obtain the desired target product.
[0052] Embodiment 11:
[0053] As described in Example 10, except that the amount of azobisisobutyronitrile added was 0.08 parts.
[0054] Comparative Example 1:
[0055] Add 10 parts of acrylamide, 2 parts of acrylic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid and 86 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.5 g of ammonium persulfate is added, and the reaction is carried out for 6 hours. The product is dried and crushed to obtain.
[0056] Comparative Example 2:
[0057] Add 10 parts of N,N-dimethylacrylamide, 2 parts of acrylic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid, 2 parts of styrene and 84 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.4 g of ammonium persulfate is added, and the reaction is carried out for 6 hours. The product is dried and crushed to obtain.
[0058] Comparative Example 3:
[0059] Add 10 parts of N,N-dimethylacrylamide, 2 parts of dodecyldimethylallyl ammonium chloride and 88 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.2 g of ammonium persulfate is added, and the reaction is carried out for 6 hours. The product is dried and crushed to obtain.
[0060] Comparative Example 4:
[0061] 1 part of nano-silica modified with γ-methacryloxypropyltrimethoxysilane, 10 parts of N,N-dimethylacrylamide, 4 parts of octadecyldimethylallyl ammonium chloride and 85 parts of deionized water are added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.5 g of ammonium persulfate is added, the reaction is carried out for 6 hours, and the product is dried and crushed to obtain.
[0062] Comparative Example 5:
[0063] 1 part of nano-silica modified with γ-methacryloxypropyltrimethoxysilane, 6 parts of N,N-dimethylacrylamide, 4 parts of vinylpyrrolidone, 4 parts of octadecyldimethylallylammonium chloride and 85 parts of deionized water are added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.5 parts of ammonium persulfate are added, the reaction is carried out for 6 hours, and the product is dried and crushed to obtain.
[0064] Comparative Example 6:
[0065] Add 2.5 parts of acrylamide, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 2.5 parts of vinyl pyrrolidone and 90 parts of N,N-dimethylformamide into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, stir at high speed, and after all the raw materials are evenly dispersed and nitrogen is continuously passed for 30 minutes, 0.5 parts of γ-methacryloxypropyltrimethoxysilane is added dropwise, and 0.04 parts of (NH4)2S2O8 and 0.04 parts of NaHSO3 are added, and stirring is continued under nitrogen protection. React for 9 hours to obtain a white gel, which is poured into a large amount of acetone and soaked for 24 hours, filtered, and extracted with methanol to remove unreacted monomers to obtain.
[0066] Comparative Example 7:
[0067] 1 part of nano-silica, 4 parts of N,N-dimethylacrylamide, 2 parts of styrene, 4 parts of hexadecyldimethylallyl ammonium chloride, 0.5 parts of vinyltrimethoxysilane and 83 parts of toluene were added into a three-necked glass bottle equipped with a nitrogen tube, a stirrer and a condenser, and stirred at high speed. After all the raw materials were evenly dispersed, nitrogen was introduced for 30 minutes, 0.25 parts of azobisisobutyronitrile were added, the heating temperature was maintained at 65°C, and after reacting for 6 hours, the product was washed with acetone and ethanol in turn, and then dried and crushed to obtain the desired target product.
[0068] Comparative Example 8:
[0069] 1 part of nano-silica, 4 parts of N,N-dimethylacrylamide, 2 parts of styrene, 4 parts of hexadecyldimethylallyl ammonium chloride, 4 parts of vinyltrimethoxysilane and 83 parts of toluene were added into a three-necked glass bottle equipped with a nitrogen tube, a stirrer and a condenser, and stirred at high speed. After all the raw materials were evenly dispersed, nitrogen was introduced for 30 minutes, 0.15 parts of ammonium persulfate were added, and the heating temperature was maintained at 65°C. After reacting for 6 hours, the product was washed with acetone and ethanol in turn, and then dried and crushed to obtain the desired target product. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0071] Figure 1 This is a graph showing the influence of Example 7 (dosage is 1% of the dry cement ash weight) in Test Example 3 of the present invention, Comparative Example 1 (dosage is 1% of the dry cement ash weight) and no addition of fluid loss additive on the sedimentation stability of cement slurry at 250°C.
[0072] Performance Evaluation
[0073] Test Example 1:
[0074] For Examples 1 to 11 and Comparative Examples 1 to 8, according to the relevant provisions of the petroleum and natural gas industry standard SY / T5504.2-2013 "Evaluation Methods for Oil Well Cement Admixtures Part 2: Fluid Loss Additives" and the national standard GB / T19139-2012 "Test Methods for Oil Well Cement", the API water loss of cement slurry was tested at different experimental temperatures and fluid loss additive dosages, and the results are shown in Table 1.
[0075] The cement slurry formula is: 500g Jiahua G grade cement + 50% 200 mesh silica sand + 5% retarder + X% fluid loss reducer + water-cement ratio of 0.53.
[0076] Among them, the retarder is homemade in the laboratory, which is a carboxylic acid retarder with a temperature resistance of up to 260°C.
[0077] Table 1 Water loss reduction performance of different water loss reducers under different conditions
[0078]
[0079]
[0080]
[0081]
[0082]
[0083]
[0084]
[0085] As can be seen from Table 1, compared with the comparative example, the fluid loss reducers prepared by Examples 1-11 of the present invention have good fluid loss reduction performance at 150 to 250°C. As the temperature increases, although the water loss of Example 1 increases, the overall water loss reduction performance remains good. At the same time, as the amount of addition increases, a good water loss reduction effect can be achieved at about 1% addition, indicating that the fluid loss reducer has excellent temperature resistance and can effectively maintain adsorption on the surface of cement particles. Comparison of different embodiments also found that the polymer monomer has a certain influence on the performance of the product, but the overall API water loss is less than 50mL. Comparing the salt resistance of the embodiments and the comparative examples, it is found that the fluid loss reducer designed by the present invention can resist the shielding effect of salt ions and still has a good water loss reduction effect at saturated salt water concentration. This is mainly because the fluid loss reducer and cement particles mainly use the condensation of silanol and silanol on the surface of cement particles, rather than conventional electrostatic adsorption, which can effectively reduce the influence of salt ions on the performance of the fluid loss reducer.
[0086] Test Example 2:
[0087] For Examples 1 to 11 and Comparative Examples 1 to 8, the compressive strength test, thickening time and other test standards in the national standard GB / T19139-2012 "Test Methods for Oil Well Cement" were used to investigate their effects on cement slurry performance and compatibility, and the results are shown in Table 2. The compressive strength of the cement slurry system without the addition of a fluid loss additive was 53 MPa, and the thickening time was 518 min.
[0088] The cement slurry formula is: 500g Jiahua G grade cement + 50% 200 mesh silica sand + 5% retarder + X% fluid loss reducer + water-cement ratio of 0.53.
[0089] The retarder is homemade in the laboratory and is a carboxylic acid retarder with a temperature resistance of up to 260°C.
[0090] Table 2 Effect of different fluid loss reducers on cement compressive strength and thickening time
[0091]
[0092]
[0093] From Table 2, it can be seen that the fluid loss reducers prepared in Examples 1-11 of the present invention have no obvious effect on the compressive strength and thickening time of cement slurry. Compared with the comparative example, since the fluid loss reducers of the present invention do not carry carboxylic acid groups, they are not easy to produce competitive adsorption with conventional carboxylic acid retarders, and can effectively reduce the effect of the fluid loss reducer on the retarding time.
[0094] Test Example 3:
[0095] For the provided fluid loss reducer Example 7 (dosage is 1% of the dry ash weight of cement) and Comparative Example 1 (dosage is 1% of the dry ash weight of cement), a cement slurry stability test was conducted in accordance with the national standard GB / T19139-2012 "Test Methods for Oil Well Cement", and the test temperature was 250°C. The sedimentation stability of Example 7 and Comparative Example 1 was compared with that of the cement sample without adding fluid loss reducer. Figure 1 shown.
[0096] Depend on Figure 1 It can be seen that after curing at 250°C, the sample without fluid loss agent has a large difference in density between the free liquid and cement paste. Compared with Comparative Example 1, the free liquid amount in Example 7 is reduced from 15.5 mL to 0 mL, and the density difference between the upper and lower cement pastes is reduced to 0.025 g / cm 3 It can be seen that the fluid loss agent provided by the present invention can effectively improve the sedimentation stability of cement slurry in an ultra-high temperature environment. Compared with the comparative example, relying on the strong interaction between organosilicon and the surface of cement particles and its own high temperature resistance, the fluid loss agent and cement particles still maintain a good polymer grid structure in an ultra-high temperature environment, maintain the viscosity of the cement slurry, effectively suspend the cement particles, and improve the sedimentation stability of the cement slurry in an ultra-high temperature environment.
[0097] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of patent protection of this application shall still be based on the scope defined in the attached claims.
Claims
1. A method for preparing an organosilicon fluid loss additive for cementing, comprising the following steps: A certain amount of nanoparticles, nonionic monomers, cationic monomers and organosilicon are added to a three-necked glass bottle equipped with a stirrer and a condenser, and an appropriate amount of toluene is added as a solvent, and stirred at a high speed. After all the raw materials are evenly dispersed, nitrogen is introduced for 30 minutes to deoxygenate, and an azo initiator is added. The mixture is heated and maintained at a certain temperature. After a period of reaction, the mixture is washed with acetone and ethanol in turn, and the product is dried and crushed to obtain the desired target product. The nonionic monomer is one of N,N-dimethylacrylamide, N,N-dimethylacrylamide and vinyl pyrrolidone, and N,N-dimethylacrylamide and styrene, wherein the mass ratio of vinyl pyrrolidone to N,N-dimethylacrylamide is 1:(1.5-3), and the mass ratio of styrene to N,N-dimethylacrylamide is 1:(2-4); The cationic monomer is one of dodecyl dimethyl allyl ammonium chloride, tetradecyl dimethyl allyl ammonium chloride, hexadecyl dimethyl allyl ammonium chloride and octadecyl dimethyl allyl ammonium chloride; The organosilicon is one of γ-methacryloxypropyltrimethoxysilane (KH570), vinyltrimethoxysilane and allyltrimethylsilane; The azo initiator is one of azobisisobutylamidine hydrochloride, azobisisobutylonitrile, azobisisobutylimidazoline hydrochloride, and azobisisoheptanenitrile; The nanoparticles are selected from the group consisting of nano silicon dioxide, nano calcium carbonate, nano calcium silicate and nano bentonite.
2. The method for preparing an organosilicon fluid loss additive for cementing according to claim 1, characterized in that: The monomer concentration is 15-30% of the total mass.
3. The method for preparing an organosilicon fluid loss additive for cementing according to claim 1, characterized in that: The mass ratio of the nanoparticles, the nonionic monomer, the cationic monomer and the organosilicon is 1:(1-12):(1-8):(1-3).
4. The method for preparing an organosilicon fluid loss additive for cementing according to claim 1, characterized in that: The azo initiator accounts for 0.1 to 1.2% of the total mass of the monomers.
5. The method for preparing an organosilicon fluid loss additive for cementing according to claim 1, characterized in that: The temperature is controlled at 50-65°C and the polymerization reaction time is 5-8h.
Citation Information
Patent Citations
Preparation method of high-temperature-resistant salt-tolerant fluid loss agent composition
CN115404061A
Constant-rheology micro-expansion fluid loss agent
CN116731262A
Preparation method of temperature-resistant and salt-resistant filter loss reducing agent for water-based drilling fluid
CN108059950A
Inorganic-organic polymer oil well cement filtrate loss reduction additive, and preparation method and application thereof
CN109503782A
Salt-responsive high-temperature-resistant zwitterionic polymer filtrate reducer and preparation method and application thereof
CN112011318A