Dispersing agent, preparation method thereof and gypsum

Through the transesterification reaction of isooctanol-capped poly12-hydroxystearic acid with fluorocarbon groups and silicate ester containing fluorocarbon groups, a dispersant with both dispersion and defoaming properties was prepared, which solved the fluidity and foam in gypsum preparation. The problem has improved the fluidity and flame retardant properties of gypsum to meet the multiple performance needs of building materials.

CN118978680AInactive Publication Date: 2024-11-19HUNAN CONSTR ENG HUIJIAN NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411072655.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, it is difficult to have additives with excellent dispersion and defoaming properties during the preparation of gypsum, resulting in poor fluidity of gypsum products and excessive foam generation, affecting product quality.

Method used

The poly12-hydroxystearic acid with isooctanol-capped polyesterification reaction was carried out with fluorocarbon group-containing silicate to prepare a dispersant with excellent dispersion and defoaming properties, through the anchoring group and The covalent bonds on the surface of gypsum particles form chelation adsorption, affecting the progress of hydration reaction and surface tension, and achieving dispersion and defoaming effects.

Benefits of technology

This dispersant significantly improves the fluidity of the gypsum and the stability of the slurry, reduces foam generation, enhances the flame retardant performance of the gypsum, and meets the demand for fire and sound insulation performance of building materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of building material additives, in particular to a dispersing agent, a preparation method of the dispersing agent and gypsum. The invention relates to a dispersing agent, which is obtained by reaction of isooctanol-terminated poly12-hydroxystearic acid and silicate ester containing a fluorocarbon group, and the molar ratio of the isooctanol-terminated poly12-hydroxystearic acid to the silicate ester containing the fluorocarbon group is (1.5-2.5): 1. The dispersing agent disclosed by the invention has excellent dispersing performance, defoaming performance and flame-retardant performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of building material additives, and more specifically, to a dispersant and a preparation method thereof, and gypsum. Background Art

[0002] Gypsum is a sulfate substance, mainly a hydrate of calcium sulfate. When gypsum is heated, the crystal water will be released, which will cause the gypsum body to change and become sintered gypsum. Sintered gypsum has excellent fire resistance, sound insulation, heat insulation and structural strength, so it is widely used in construction, medical, industry and other fields.

[0003] When preparing gypsum, the solidification of gypsum will form a crystal network, but an overly dense crystal network will lead to poor fluidity of the gypsum, which will make it difficult to shape or pour the gypsum. The addition of dispersants can break up this crystal network to a certain extent, making the gypsum easier to flow and handle, thereby improving the quality of gypsum products. In addition, when preparing gypsum, in order to obtain more functional effects, auxiliary additives are usually added to the gypsum, and even some organic matrices are added. However, the use of auxiliary additives and organic matrices is likely to cause excessive foam generation, thereby affecting the quality of gypsum products, and defoamers can effectively improve the generation of foam.

[0004] However, currently, dispersants and defoamers are separate products, and need to be added separately when preparing gypsum products. In order to improve the market competitiveness of products, an additive with both excellent dispersing properties and defoaming properties is urgently needed for use in gypsum preparation. Summary of the invention

[0005] In order to improve the defect that conventional additives are difficult to have both excellent dispersibility and defoaming performance, the present application provides a dispersant and a preparation method thereof, and gypsum.

[0006] In the first aspect, the present application provides a dispersant, which adopts the following technical solution:

[0007] A dispersant is obtained by reacting isooctyl alcohol-terminated poly 12-hydroxystearic acid with a silicate containing a fluorocarbon group, wherein the molar ratio of the isooctyl alcohol-terminated poly 12-hydroxystearic acid to the silicate containing a fluorocarbon group is (1.5-2.5):1.

[0008] There is a consistent correspondence between the dispersion performance of polymer on gypsum and the hardening and setting time of gypsum, and the setting time reflects the degree of hydration reaction of gypsum. That is to say, the dispersion of polymer on gypsum is achieved by affecting the progress of hydration reaction of gypsum, and the degree of influence of polymer on hydration reaction of gypsum depends on the strength of adsorption of copolymer on the surface of gypsum particles.

[0009] Specifically, when there are anchoring groups on the polymer, the anchoring groups will form covalent bonds with the surface of the gypsum particles, thereby achieving chelation and adsorption, which will reduce the contact opportunities between water molecules and gypsum particles, slow down the hydration reaction of the gypsum and prolong the coagulation time, slow down the hardening and coagulation speed of the gypsum, and improve the fluidity of the slurry, thereby showing an excellent dispersion effect.

[0010] Among the anchoring groups, the electronegativity of the silicate group is very close to that of the hydroxyl group. The smaller the electronegativity difference, the stronger the covalency of the bond and the stronger the bond. In other words, the selection of silicate can promote a better dispersion effect of gypsum.

[0011] The isooctyl alcohol-terminated poly 12-hydroxystearic acid has excellent polarity, which can help gypsum powder to be evenly dispersed in the liquid phase to form a stable dispersion system. It also has the effect of reducing surface tension. Therefore, when the isooctyl alcohol-terminated poly 12-hydroxystearic acid is combined with a fluorocarbon group-containing silicate and undergoes an ester exchange reaction, the dispersant will have an extra flexible chain, thereby forming good compatibility with the dispersion medium, fully extending in the dispersion medium, and thereby obtaining a better dispersion effect.

[0012] In addition, since the fluorocarbon-containing silicate contains fluorocarbon groups, the surface activity of the fluorocarbon groups can hinder the formation and aggregation of bubbles, thereby playing a defoaming role. The fluorocarbon groups can also reduce the surface tension of the liquid, making the bubbles easy to break and disperse, thereby slowing down the aggregation of bubbles and the generation of foam.

[0013] In summary, when the isooctyl alcohol-terminated poly 12-hydroxystearic acid is combined with a fluorocarbon group-containing silicate and subjected to an ester exchange reaction, the prepared dispersant will have both better dispersing and defoaming properties.

[0014] Preferably, the preparation method of the isooctyl alcohol-terminated poly 12-hydroxystearic acid comprises the following steps:

[0015] Synthesis of Poly 12-Hydroxystearic Acid:

[0016] 12-hydroxystearic acid, antioxidant DLTP, antioxidant 1010 and catalyst-stannous octoate are sequentially added to the solvent xylene, and heated to 90-110° C. while stirring under nitrogen. After complete dissolution, the temperature is gradually raised to 160-180° C., and condensation reflux is maintained, and the generated water is separated through a water separator. When the acid value reaches 30-33 mgKOH / g, the reaction is stopped to obtain poly-12-hydroxystearic acid;

[0017] Poly 12-hydroxystearic acid end-capped:

[0018] The poly 12-hydroxystearic acid and isooctyl alcohol are mixed in a molar ratio of 1:(1.0-1.4), and the temperature is raised to 160-180° C. while stirring under nitrogen. When the acid value reaches 5.8-6.2 mgKOH / g, water and solvent in the product are removed by reduced pressure distillation, and vacuum drying is performed to obtain isooctyl alcohol-terminated poly 12-hydroxystearic acid.

[0019] Preferably, the poly 12-hydroxystearic acid comprises the following raw materials in parts by weight: 95-105 parts of 12-hydroxystearic acid, 0.2-0.5 parts of antioxidant DLTP, 0.2-0.5 parts of antioxidant 1010 and 0.01-0.2 parts of catalyst-stannous octoate.

[0020] Preferably, the silicate containing fluorine carbon groups is obtained by reacting a silicate containing hydroxy groups with trifluoroacetic acid.

[0021] Preferably, the hydroxyl-containing silicate is obtained by reacting tris(2,3-dichloropropyl)methyl silicate with trishydroxymethylphosphine oxide.

[0022] When gypsum is used in the construction field, flame retardant performance is also one of the key points of building materials. In the present application, the hydroxy silicate is obtained by reacting tris(2,3-dichloropropyl)methyl silicate with trihydroxymethylphosphine oxide, and chlorine is precipitated in the subsequent substitution reaction. Therefore, the final dispersant will contain both silicon and phosphorus elements, thereby forming a silicon-phosphorus synergistic flame retardant system.

[0023] Among them, the flame retardant mechanism of the silicon-phosphorus synergistic flame retardant system is that the silicon element can play a flame retardant role by hindering heat conduction and mass transfer during the combustion process, thereby forming a layer of silicon carbide protective layer to slow down the combustion rate, while the phosphorus element can play a flame retardant role by promoting the formation of a carbonized layer and improving the carbon soot structure, increasing the carbonization degree of the carbon soot and preventing the entry of oxygen and heat.

[0024] When silicon and phosphorus are used together, silicon can promote the decomposition and activation of phosphorus, thereby improving the effect of phosphorus in the combustion process. At the same time, phosphorus can also improve the reactivity and effect of silicon, thereby forming a synergistic flame retardant effect.

[0025] Preferably, the preparation method of the hydroxyl-containing silicate comprises the following steps:

[0026] Preparation of tri(2,3-dichloropropyl)methylsilicate:

[0027] Methyltrimethoxysilane and dichloropropanol are mixed with a solvent-xylene in a molar ratio of 1:4, and then the temperature is raised to 100-106° C., and the methanol obtained by the reaction is distilled out through a fractionator, and then the temperature is raised to 140-150° C. until the theoretical value of methanol is distilled out, and finally the solvent and excess dichloropropanol are distilled out, and cooled to obtain tri(2,3-dichloropropyl)methylsilicate;

[0028] Preparation of hydroxyl silicate:

[0029] Under a nitrogen atmosphere, 0.12-0.18 mol of trimethylolphosphine oxide and 50-70 ml of diethylene glycol dimethyl ether are mixed in a four-necked flask, and then a hydrogen chloride absorption device and a drying tank are installed on a reflux condenser, and 0.4-0.6 mol of tri(2,3-dichloropropyl)methylsilicate is slowly added at a temperature of 20° C. After the addition is completed, the temperature is raised to 60-80° C., and the reaction is kept warm for 6-8 hours, and then the temperature is raised to 110-130° C., and the reaction is kept warm for 4-6 hours, and then 0.8-0.9 g of an acid binding agent triethylamine is added, and after stirring for 1 hour, the mixture is filtered and distilled, and two times the volume of deionized water is added, and then a sodium carbonate solution with a total mass of 5wt% is added dropwise until the pH is 7, and the mixture is allowed to stand for stratification, and the lower layer of liquid is taken and dried to obtain a hydroxy-containing silicate.

[0030] In the above system, two hydroxyl groups in tris(hydroxymethyl)phosphine oxide react with two chlorine groups in tris(2,3-dichloropropyl)methylsilicate and precipitate, thereby connecting the main chains of the two to form a silicate system containing one active hydroxyl group.

[0031] Preferably, the preparation method of the fluorocarbon group-containing silicate is:

[0032] The trifluoroacetic acid and the hydroxyl-containing silicate are mixed in dimethyl sulfoxide at a molar ratio of (2-4):1, and the dimethyl sulfoxide is added in a three-fold volume amount, and then concentrated sulfuric acid of 3wt% of the total mass is added, and an esterification reaction is carried out at 60-80°C, and the generated water is separated by a water separator. When the pH value reaches 7, the reaction is terminated to obtain a fluorocarbon group-containing silicate.

[0033] The carboxyl group on trifluoroacetic acid and the hydroxyl group on the hydroxyl-containing silicate undergo an esterification reaction under the catalysis of concentrated sulfuric acid and temperature, thereby connecting the fluorocarbon group to the silicate main chain.

[0034] In a second aspect, the present application provides a method for preparing a dispersant, using the following technical solution:

[0035] A method for preparing a dispersant comprises the following steps: mixing isooctyl alcohol-terminated poly-12-hydroxystearic acid with a silicate containing a fluorocarbon group, reacting the mixture at 80-100°C for 2 hours, vacuuming the mixture for 1 hour to remove small molecules, and finally obtaining the dispersant.

[0036] In the above system, the poly-12-hydroxystearic acid terminated with isooctyl alcohol undergoes an ester exchange reaction with the silicate containing a fluorocarbon group, thereby connecting the main chains of the two.

[0037] In a third aspect, the present application provides a gypsum, which adopts the following technical solution:

[0038] A kind of gypsum, wherein the gypsum is made of the above-mentioned dispersant.

[0039] In summary, this application has the following beneficial effects:

[0040] 1. When there are anchoring groups on the polymer, the anchoring groups will form covalent bonds with the surface of gypsum particles, thereby achieving chelation and adsorption, which will reduce the contact opportunities between water molecules and gypsum particles, slow down the hydration reaction of gypsum and prolong the coagulation time, slow down the hardening and coagulation speed of gypsum, and improve the fluidity of the slurry, thus showing an excellent dispersion effect. Among the anchoring groups, the electronegativity of the silicate group is very close to that of the hydroxyl group, and the smaller the electronegativity, the stronger the covalent nature of the bond and the stronger the bond. In other words, the selection of silicate can promote gypsum to have a better dispersion effect.

[0041] 2. The isooctyl alcohol-terminated poly 12-hydroxystearic acid has excellent polarity, which can help gypsum powder to be evenly dispersed in the liquid phase to form a stable dispersion system. It also has the effect of reducing surface tension. Therefore, when the isooctyl alcohol-terminated poly 12-hydroxystearic acid is combined with a fluorocarbon group-containing silicate and undergoes an ester exchange reaction, the dispersant will have an extra flexible chain, thereby forming good compatibility with the dispersion medium, fully stretching in the dispersion medium, and thus obtaining a better dispersion effect.

[0042] 3. Since the fluorocarbon-containing silicate contains fluorocarbon groups, the surface activity of the fluorocarbon groups can hinder the formation and aggregation of bubbles, thereby playing a defoaming role. In addition, the fluorocarbon groups can also reduce the surface tension of the liquid, making the bubbles easy to break and disperse, thereby slowing down the aggregation of bubbles and the generation of foam.

[0043] 4. When gypsum is used in the construction field, flame retardant performance is also one of the key points of building materials. In this application, the hydroxy silicate is obtained by reacting tris(2,3-dichloropropyl)methyl silicate with trihydroxymethylphosphine oxide, and chlorine is precipitated in the subsequent substitution reaction. Therefore, the final dispersant will contain both silicon and phosphorus elements, thereby forming a silicon-phosphorus synergistic flame retardant system. DETAILED DESCRIPTION

[0044] The present application is further described in detail below in conjunction with Examples 1-3 and Comparative Examples 1-4.

[0045] raw material

[0046] 12-Hydroxystearic acid CAS: 106-14-9; Antioxidant DLTP; Antioxidant 1010; Stannous octoate CAS: 301-10-0; Xylene CAS: 1330-20-7; Isooctanol CAS: 26952-12-6; Tris(hydroxymethyl)phosphine oxide CAS: 1067-12-5; Methyltrimethoxysilane CAS: 1185-55-3; Dichloropropanol CAS: 96-23-1 ; Diethylene glycol dimethyl ether CAS: 111-96-6; Triethylamine CAS: 121-44-8; Trifluoroacetic acid CAS: 76-05-1; Dimethyl sulfoxide CAS: 67-68-5; Tetraethyl silicate CAS: 78-10-4; Gypsum powder and Chang gypsum; Polyvinyl alcohol CAS: 9002-89-5; Methyl cellulose CAS: 9004-67-5; Sodium citrate CAS: 6132-04-3.

[0047] Example

[0048] Example 1

[0049] A dispersant obtained by reacting poly-12-hydroxystearic acid terminated with isooctanoic acid with a silicate containing a fluorocarbon group;

[0050] The preparation method of the dispersant is as follows: poly 12-hydroxystearic acid terminated with isooctyl alcohol is mixed with silicate containing fluorocarbon groups, wherein the molar ratio of poly 12-hydroxystearic acid terminated with isooctyl alcohol to silicate containing fluorocarbon groups is 2:1, followed by reacting at 90°C for 2h, vacuuming for 1h to remove small molecules, and finally obtaining the dispersant.

[0051] The preparation method of isooctanoic acid-terminated poly 12-hydroxystearic acid comprises the following steps:

[0052] Synthesis of Poly 12-Hydroxystearic Acid:

[0053] 100g 12-hydroxystearic acid, 0.35g antioxidant DLTP, 0.35g antioxidant 1010 and 0.1g catalyst-stannous octoate are sequentially added to 200ml solvent xylene, and heated to 100°C while stirring under nitrogen. After complete dissolution, the temperature is gradually raised to 170°C, and condensation reflux is maintained, and the generated water is separated by a water separator. When the acid value reaches 32.5mgKOH / g, the reaction is stopped to obtain poly 12-hydroxystearic acid;

[0054] Poly 12-hydroxystearic acid end-capped:

[0055] Poly 12-hydroxystearic acid and isooctyl alcohol were mixed in a molar ratio of 1:1.2, and the temperature was raised to 170°C while stirring under nitrogen. When the acid value reached 6.0 mgKOH / g, water and solvent in the product were removed by reduced pressure distillation, and vacuum drying was performed to obtain isooctyl alcohol-terminated poly 12-hydroxystearic acid.

[0056] The silicate containing fluorocarbon groups is obtained by reacting hydroxy silicate with trifluoroacetic acid. The preparation method of the silicate containing fluorocarbon groups is as follows: trifluoroacetic acid and hydroxy silicate are mixed in dimethyl sulfoxide at a molar ratio of 3:1, and dimethyl sulfoxide is added in a three-fold volume amount, and then 3wt% of concentrated sulfuric acid is added to carry out esterification at 70°C, and the generated water is separated by a water separator. When the pH value reaches 7, the reaction is terminated to obtain the silicate containing fluorocarbon groups.

[0057] The preparation method of hydroxyl silicate comprises the following steps:

[0058] Preparation of tri(2,3-dichloropropyl)methylsilicate:

[0059] Methyltrimethoxysilane and dichloropropanol are mixed with three times the volume of solvent-xylene in a molar ratio of 1:4, and then the temperature is raised to 0.4°C, and the methanol obtained by the reaction is distilled out through a fractionator, and then the temperature is raised to 145°C until the theoretical value of methanol is distilled out, and finally the solvent and excess dichloropropanol are distilled out, and cooled to obtain tri(2,3-dichloropropyl)methylsilicate;

[0060] Preparation of hydroxyl silicate:

[0061] Under a nitrogen atmosphere, 0.15 mol of trimethylolphosphine oxide and 60 ml of diethylene glycol dimethyl ether solvent were mixed in a four-necked flask, and then a hydrogen chloride absorption device and a drying tank were installed on the reflux condenser, and 0.5 mol of tri(2,3-dichloropropyl)methylsilicate was slowly added at a temperature of 20°C. After the addition was completed, the temperature was raised to 70°C, and the reaction was kept warm for 7 hours, and then the temperature was raised to 120°C, and the reaction was kept warm for 4-6 hours, and then 0.85 g of acid binding agent triethylamine was added, and after stirring for 1 hour, suction filtration and distillation were performed, and two volumes of deionized water were added, and then a sodium carbonate solution with a total mass of 5wt% was added dropwise until the pH was 7, and the layer was allowed to stand for stratification, and the lower layer of liquid was taken and dried to obtain a hydroxy-containing silicate.

[0062] Example 2-3

[0063] The difference from Example 1 is that the molar ratio of the poly 12-hydroxystearic acid terminated with isooctyl alcohol to the silicate containing fluorocarbon groups is different, as shown in Table 1.

[0064] Table 1 Molar ratio of each component of the dispersant of Examples 1-3

[0065] Example 1 Example 2 Example 3 Poly(12-hydroxystearic acid) terminated with isooctyl alcohol 2 1 3 Fluorocarbon-containing silicates 1 1 1

[0066] Comparative Example

[0067] Comparative Example 1

[0068] The difference from Example 1 is that the poly 12-hydroxystearic acid terminated with isooctyl alcohol is no longer added.

[0069] Comparative Example 2

[0070] The difference from Example 1 is that the silicate containing fluorocarbon groups is replaced by silicate containing hydroxyl groups in the same amount.

[0071] Comparative Example 3

[0072] The difference from Comparative Example 2 is that the hydroxyl-containing silicate is replaced by tetraethyl silicate in the same amount.

[0073] Application Examples

[0074] Application Examples 1-3

[0075] A gypsum board comprises the following raw materials: 60 g of gypsum powder, 2 g of polyvinyl alcohol, 4 g of methyl cellulose, 1 g of sodium citrate, 3 g of the dispersant of Examples 1-3 and 100 g of water;

[0076] The preparation method of the gypsum board is as follows: polyvinyl alcohol, methyl cellulose, sodium citrate, a dispersant and water are mixed, stirred evenly, and then gypsum powder is added and stirred again to obtain a slurry; the slurry is then made into a slab, pressurized at 0.3 MPa for 30 minutes, and then placed at 30°C and 0.2 MPa for 13 hours, dried at 40°C for 30 hours, and maintained at 25°C for 8 days to obtain a gypsum board.

[0077] Application comparison

[0078] Application Comparative Example 1

[0079] The difference from Application Example 1 is that no dispersant is used.

[0080] Application Comparative Examples 2-4

[0081] The difference from Application Example 1 is that the dispersant is selected from Comparative Examples 1-3.

[0082] Performance testing

[0083] Detection Methods

[0084] 1. Dispersion performance test

[0085] Three sample slurries were taken out from application examples 1-3 and application comparative examples 1-2, and then the initial diffusion of the samples was tested and the average value was taken according to GB / T8077-2000 "Test method for uniform placement of concrete admixtures". The initial diffusion was used to define the fluidity of the sample and to characterize the dispersion effect.

[0086] The test data are shown in Table 2.

[0087] Table 2 Dispersion effect of application examples 1-3 and comparative examples 1-2

[0088] Initial diffusion / mm Initial diffusion / mm Application Example 1 289 Application Comparative Example 1 173 Application Example 2 280 Application Comparative Example 2 275 Example 3 282

[0089] 2. Defoaming performance test

[0090] Three sample gypsum boards were taken out from application comparative examples 2-3 respectively, and then the amount of bubbles on the surface of the samples was determined by observation. The defoaming effect was determined by the amount of bubbles. The test data are shown in Table 3.

[0091] Table 3 Defoaming effect of comparative example 2-3

[0092] Bubble volume Bubble volume Application Comparative Example 2 less Application Comparative Example 3 More

[0093] 3. Flame retardant performance test

[0094] Three sample gypsum boards were taken out from application comparative examples 3-4 respectively, and then the limiting oxygen index of the samples was tested by a JF-3 oxygen index meter, and the average value was taken. The test data is shown in Table 4.

[0095] Table 4 Flame retardant properties of comparative examples 3-4

[0096] Limiting oxygen index Limiting oxygen index Application Comparative Example 3 34 Application Comparative Example 4 31

[0097] Referring to Application Example 1 and Application Comparative Examples 1-2 and in combination with Table 2, it can be seen that the initial diffusion degree of Application Comparative Example 1 is significantly reduced compared with Application Example 1; and the initial diffusion degree of Application Comparative Example 2 is still slightly reduced compared with Application Example 1, which shows that the use of silicates containing fluorocarbon groups can effectively improve the dispersion properties of gypsum, and when the silicates containing fluorocarbon groups are used in combination with isooctyl alcohol-terminated poly 12-hydroxystearic acid, the dispersion properties of gypsum will be further improved.

[0098] The reason is that there is a consistent correspondence between the dispersion performance of polymer on gypsum and the hardening and setting time of gypsum, and the setting time reflects the degree of hydration reaction of gypsum. In other words, the dispersion of polymer on gypsum is achieved by affecting the progress of hydration reaction of gypsum, and the degree of influence of polymer on hydration reaction of gypsum depends on the strength of adsorption of copolymer on the surface of gypsum particles.

[0099] Specifically, when there are anchoring groups on the polymer, the anchoring groups will form covalent bonds with the surface of the gypsum particles, thereby achieving chelation and adsorption, which will reduce the contact opportunities between water molecules and gypsum particles, slow down the hydration reaction of the gypsum and prolong the coagulation time, slow down the hardening and coagulation speed of the gypsum, and improve the fluidity of the slurry, thereby showing an excellent dispersion effect.

[0100] Among the anchoring groups, the electronegativity of the silicate group is very close to that of the hydroxyl group. The smaller the electronegativity difference, the stronger the covalency of the bond and the stronger the bond. In other words, the selection of silicate can promote a better dispersion effect of gypsum.

[0101] The isooctyl alcohol-terminated poly 12-hydroxystearic acid has excellent polarity, which can help gypsum powder to be evenly dispersed in the liquid phase to form a stable dispersion system. It also has the effect of reducing surface tension. Therefore, when the isooctyl alcohol-terminated poly 12-hydroxystearic acid is combined with a fluorocarbon group-containing silicate and undergoes an ester exchange reaction, the dispersant will have an extra flexible chain, thereby forming good compatibility with the dispersion medium, fully stretching in the dispersion medium, and thereby obtaining a better dispersion effect.

[0102] In summary, when the isooctyl alcohol-terminated poly 12-hydroxystearic acid is combined with a fluorocarbon group-containing silicate and subjected to an ester exchange reaction, the prepared dispersant will have better dispersing properties for gypsum.

[0103] Referring to Application Examples 1-3 and in combination with Table 2, it can be seen that the initial diffusion degrees of Application Examples 2-3 are slightly reduced compared with Application Example 1, which indicates that when the molar ratio of isooctyl alcohol-capped poly 12-hydroxystearic acid and fluorocarbon group-containing silicate is used in Application Example 1, the prepared dispersant will have a better dispersion effect on gypsum.

[0104] Referring to application examples 2-3 and combining with Table 3, it can be seen that the amount of bubbles in application example 3 is significantly increased compared with application example 2, which indicates that the presence of fluorocarbon groups can effectively improve the generation of bubbles.

[0105] The reason is that the surface active effect of the fluorocarbon group can hinder the formation and aggregation of bubbles, thereby playing a defoaming role. In addition, the fluorocarbon group can also reduce the surface tension of the liquid, making the bubbles easy to break and disperse, thereby slowing down the aggregation of bubbles and the generation of foam.

[0106] Referring to application examples 3-4 and combining with Table 4, it can be seen that the limiting oxygen index of application example 4 is significantly reduced compared with that of application example 3, which shows that compared with the use of tetraethyl silicate, the use of the hydroxyl silicate of the present application can promote gypsum to have better flame retardant properties.

[0107] The reason is that the hydroxy silicate is obtained by the reaction of tri(2,3-dichloropropyl)methyl silicate and trihydroxymethylphosphine oxide, and chlorine is precipitated in the subsequent substitution reaction. Therefore, the final dispersant will contain both silicon and phosphorus elements, thus forming a silicon-phosphorus synergistic flame retardant system.

[0108] Among them, the flame retardant mechanism of the silicon-phosphorus synergistic flame retardant system is that the silicon element can play a flame retardant role by hindering heat conduction and mass transfer during the combustion process, thereby forming a layer of silicon carbide protective layer to slow down the combustion rate, while the phosphorus element can play a flame retardant role by promoting the formation of a carbonized layer and improving the carbon soot structure, increasing the carbonization degree of the carbon soot and preventing the entry of oxygen and heat.

[0109] When silicon and phosphorus are used together, silicon can promote the decomposition and activation of phosphorus, thereby improving the effect of phosphorus in the combustion process. At the same time, phosphorus can also improve the reactivity and effect of silicon, thereby forming a synergistic flame retardant effect.

[0110] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A dispersant, characterized in that: The invention is obtained by reacting poly 12-hydroxystearic acid terminated with isooctyl alcohol and silicate containing fluorine carbon group, wherein the molar ratio of poly 12-hydroxystearic acid terminated with isooctyl alcohol and silicate containing fluorine carbon group is (1.5-2.5):

1.

2. The dispersant according to claim 1, characterized in that The preparation method of the isooctyl alcohol-terminated poly-12-hydroxystearic acid comprises the following steps: Synthesis of Poly 12-Hydroxystearic Acid: 12-hydroxystearic acid, antioxidant DLTP, antioxidant 1010 and catalyst-stannous octoate are sequentially added to the solvent xylene, and heated to 90-110° C. while stirring under nitrogen. After complete dissolution, the temperature is gradually raised to 160-180° C., and condensation reflux is maintained, and the generated water is separated through a water separator. When the acid value reaches 30-33 mgKOH / g, the reaction is stopped to obtain poly-12-hydroxystearic acid; Poly 12-hydroxystearic acid end-capped: The poly 12-hydroxystearic acid and isooctyl alcohol are mixed in a molar ratio of 1:(1.0-1.4), and the temperature is raised to 160-180° C. while stirring under nitrogen. When the acid value reaches 5.8-6.2 mgKOH / g, water and solvent in the product are removed by reduced pressure distillation, and vacuum drying is performed to obtain isooctyl alcohol-terminated poly 12-hydroxystearic acid.

3. The dispersant according to claim 2, characterized in that: The poly 12-hydroxystearic acid comprises the following raw materials in parts by weight: 95-105 parts of 12-hydroxystearic acid, 0.2-0.5 parts of antioxidant DLTP, 0.2-0.5 parts of antioxidant 1010 and 0.01-0.2 parts of catalyst-stannous octoate.

4. The dispersant according to claim 1, characterized in that: The fluorine-containing silicate is obtained by reacting a hydroxyl-containing silicate with trifluoroacetic acid.

5. The dispersant according to claim 4, characterized in that: The hydroxyl-containing silicate is obtained by reacting tris(2,3-dichloropropyl)methyl silicate with trishydroxymethylphosphine oxide.

6. The dispersant according to claim 5, characterized in that The preparation method of the hydroxyl silicate comprises the following steps: Preparation of tri(2,3-dichloropropyl)methylsilicate: Methyltrimethoxysilane and dichloropropanol are mixed with a solvent-xylene in a molar ratio of 1:4, and then the temperature is raised to 100-106° C., and the methanol obtained by the reaction is distilled out through a fractionator, and then the temperature is raised to 140-150° C. until the theoretical value of methanol is distilled out, and finally the solvent and excess dichloropropanol are distilled out, and cooled to obtain tri(2,3-dichloropropyl)methylsilicate; Preparation of hydroxyl-containing silicates: Under a nitrogen atmosphere, 0.12-0.18 mol of trimethylolphosphine oxide and 50-70 ml of diethylene glycol dimethyl ether are mixed in a four-necked flask, and then a hydrogen chloride absorption device and a drying tank are installed on a reflux condenser, and 0.4-0.6 mol of tri(2,3-dichloropropyl)methylsilicate is slowly added at a temperature of 20° C. After the addition is completed, the temperature is raised to 60-80° C., and the reaction is kept warm for 6-8 hours, and then the temperature is raised to 110-130° C., and the reaction is kept warm for 4-6 hours, and then 0.8-0.9 g of an acid binding agent triethylamine is added, and after stirring for 1 hour, the mixture is filtered and distilled, and two times the volume of deionized water is added, and then a sodium carbonate solution with a total mass of 5wt% is added dropwise until the pH is 7, and the mixture is allowed to stand for stratification, and the lower layer of liquid is taken and dried to obtain a hydroxy-containing silicate.

7. The dispersant according to claim 6, characterized in that The preparation method of the silicate containing fluorine carbon group is as follows: The trifluoroacetic acid and the hydroxyl-containing silicate are mixed in dimethyl sulfoxide at a molar ratio of (2-4):1, and the dimethyl sulfoxide is added in a three-fold volume amount, and then concentrated sulfuric acid of 3wt% of the total mass is added, and an esterification reaction is carried out at 60-80°C, and the generated water is separated by a water separator. When the pH value reaches 7, the reaction is terminated to obtain a fluorocarbon group-containing silicate.

8. A method for preparing the dispersant according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing poly 12-hydroxystearic acid terminated with isooctyl alcohol and silicate containing fluorocarbon groups, reacting the mixture at 80-100° C. for 2 hours, vacuuming the mixture for 1 hour to remove small molecules, and finally obtaining a dispersant.

9. A gypsum, characterized in that: The gypsum is selected from the dispersant described in any one of claims 1-7.

Citation Information

Patent Citations

  • Preparation method and use of organic fIuorosiIane waterproofing agent

    CN102161864A

  • Waterproof gypsum board and preparation method thereof

    CN118420312A

  • Magnetic fluid using poly(12-hydroxystearic acid) dispersant having acidic end

    JP1999074113A

  • Dispersant for gypsum and dispersant composition for gypsum

    JP2007320786A

  • Magnetic colloids using acid terminated poly (12-hydroxystearic acid) dispersants