Silica gel moisturizing dressing and preparation method thereof
By mixing the silicone precursor with the pore-forming agent and performing thermal curing, punching and hydrophilic modification, silicone moisturizing dressing with good adhesion and liquid absorption properties is prepared, which solves the breathability and absorption capacity of existing silicone dressings. The problem of insufficient results has achieved stable healing of wounds and reduced costs.
Patent Information
- Application Number
- CN202411064711.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The existing silicone dressings have insufficient breathability, limited absorption capacity, unstable adhesion performance, and high cost, which limits their wide application in medical environments.
By mixing the liquid silicone precursor with the pore forming agent, heat curing, removing the pore forming agent, drilling and surface hydrophilic modification, silicone moisturizing dressing with good tissue adhesion and liquid absorption properties is prepared to achieve wounds Close fit and exudate.
Silicone dressings have rich pores and provide good moisturizing and breathable function. They can fit the skin tightly on their own, avoid adhesive allergies, reduce preparation costs, and leave no disinfectant residues, improving liquid absorption performance and comfort.
Smart Images

Figure CN118978735A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical supplies, and in particular to a silicone moisturizing dressing and a preparation method thereof. Background Art
[0002] The skin is the largest organ in the human body and also the first barrier for the body to resist the external environment. It protects the body from various physical, chemical and biological factors and maintains the balance of body fluids and electrolytes. Various injury factors such as burns and trauma in life can lead to the destruction of skin structure and function. Especially for patients with large areas of skin defects, such as severe burns, the lack of skin barrier protection will lead to water and electrolyte disorders, infection, loss of energy and nutrients, thus seriously threatening human life. In clinical treatment, the application of dressings is particularly important. They provide protection for the wound surface, provide a relatively sterile and suitable moist environment, and promote wound repair.
[0003] Silicone is a polymer material with many excellent properties, including good mechanical properties, chemical stability and biocompatibility. These excellent properties make silicone an ideal material for preparing wound dressings. However, existing silicone dressings still have insufficient air permeability and limited absorption capacity, which cannot effectively absorb wound secretions, which may lead to excessive local exudate and affect wound healing; in addition, its adhesion performance is unstable and it is easy to fall off or shift, affecting the treatment effect and patient comfort; furthermore, compared with traditional dressings, silicone dressings are usually more expensive, which may limit its widespread application in certain medical environments.
[0004] Giving silicone dressings excellent breathability and absorption properties, good adhesion and low cost are key technical issues that need to be urgently addressed in their application in the field of medical dressings, which is of great significance for improving patient comfort and treatment effects. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention provides a silicone moisturizing dressing and a preparation method thereof. The silicone moisturizing dressing of the present invention is prepared by mixing a liquid silicone precursor with a pore-forming agent, washing and removing the pore-forming agent after the silicone material is thermally cured, and obtaining the silicone moisturizing dressing by punching and surface hydrophilic modification. The prepared silicone moisturizing dressing has good tissue adhesion, can fit tightly to irregular wound surfaces, absorb exudate and keep the wound base moist, and excess exudate can be discharged from the directional micropores to the surface of the hydrophilic layer of the dressing, and maintain the stability of the wound microenvironment through natural evaporation or absorption by the external dressing, thereby efficiently promoting wound healing and repair.
[0006] The technical solution of the present invention is as follows:
[0007] The first aspect of the present invention provides a method for preparing a medical silicone moisturizing dressing, comprising the following steps:
[0008] S1: Prepare silica precursor.
[0009] S2: adding a pore-forming agent into the silica gel precursor, stirring the mixture evenly to obtain a silica gel mixture.
[0010] S3: Add the silicone mixture into the mold, heat and cure it, and take it out to obtain the initial product of the silicone dressing.
[0011] S4: After washing the initial silicone dressing product, perforation and / or surface hydrophilic modification are performed.
[0012] S6: After drying and sterilization, the medical silicone moisturizing dressing is obtained.
[0013] Further, in step S1, in step S1, the silica gel precursor is purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0014] Furthermore, the silica gel precursor includes a silica gel component A and a silica gel component B. When used, the silica gel component A and the silica gel component B are mixed to obtain a silica gel precursor; wherein the mass ratio of the silica gel component A to the silica gel component B is 0.8 to 1.5:1.
[0015] Furthermore, in step S2, the pore-forming agent includes any one of potassium nitrate, ammonium sulfate, ammonium chloride, sodium chloride, potassium chloride, and sucrose particles; and the mass ratio of the pore-forming agent to the silica gel precursor is 1:1 to 3:2.
[0016] Furthermore, in step S3, the material of the mold is polymethyl methacrylate; the temperature of the heating and curing is 10 to 100° C., and the time is 0.5 to 10 hours.
[0017] Furthermore, in step S4, the washing temperature is 1 to 100° C. and the washing time is 0.5 to 10 hours.
[0018] Furthermore, in step S4, the punching is to punch holes on the surface of the washed silica gel primary product; the punching method includes one of mechanical punching and laser punching; the hole diameter of the punched hole is 0.01 to 10 mm, and the distance between adjacent holes is 0.01 to 10 mm; the shape of the punched hole includes any one of a cylinder, a cone, and an irregular body.
[0019] Furthermore, in step S4, the hydrophilic modification is performed by soaking in dopamine hydrochloride, or spraying polyvinyl alcohol or carboxymethyl cellulose after plasma surface treatment.
[0020] Furthermore, the concentration of dopamine hydrochloride is 0.1-0.5wt%; the immersion time is 12-48h; the concentration of polyvinyl alcohol is 1-10wt%; the power of the plasma surface treatment is 500-1000W, the distance is 5-15mm, and the time is 10-30s.
[0021] The second aspect of the present invention provides a medical silicone moisturizing dressing prepared by the preparation method described in the first aspect.
[0022] The beneficial technical effects of the present invention are:
[0023] (1) The silicone dressing of the present invention has abundant pores, which can provide good moisture-retaining and breathable functions for the wound surface. When the wound surface exudates too much, it can be discharged in time through the directional micropores of the material, which is beneficial to maintaining the stability of the wound surface microenvironment and promoting repair.
[0024] (2) The silicone dressing of the present invention has excellent adhesion and flexibility, and can fit closely to the skin tissue, avoiding the use of adhesives and the hazards such as allergies caused by them. At the same time, the silicone dressing can tolerate local deformation and is particularly suitable for wounds in joints and other places that require large movements. When the dressing is removed, it does not adhere to the wound tissue, greatly reducing the pain of dressing change for patients.
[0025] (3) The silicone dressing of the present invention is prepared by high-pressure steam / irradiation sterilization, so there will be no disinfectant residue, and will not cause adverse reactions such as foreign body allergy and disinfectant poisoning caused by disinfectant residue. At the same time, no water is used in the preparation process, avoiding deformation and shrinkage caused by water flow during preparation and use.
[0026] (4) The present invention improves the water absorption performance of the silicone dressing by performing hydrophilic treatment on the surface of the dressing and the inside of the pores. Compared with the untreated dressing, the average liquid absorption performance increases by about 100%.
[0027] (5) The raw materials used in the present invention are cheap, readily available and safe. The pore-forming agent used can be reused by evaporation and crystallization, thereby reducing the preparation cost and the preparation process has circular economy. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the structure of the medical silicone moisturizing dressing according to Example 3 of the present invention.
[0029] Figure 2 This is a schematic diagram of the cross-sectional structure of the medical silicone moisturizing dressing according to Example 3 of the present invention.
[0030] Figure 3 This is a schematic diagram of the structure of the medical silicone moisturizing dressing according to Example 5 of the present invention.
[0031] Figure 4This is a schematic diagram of the cross-sectional structure of the medical silicone moisturizing dressing according to Example 5 of the present invention.
[0032] Figure 5 This is a scanning electron microscope schematic diagram of the surface structure of the medical silicone moisturizing dressing according to Example 5 of the present invention.
[0033] Figure 6 These are the experimental results of cytotoxicity and blood compatibility of the medical silicone moisturizing dressing of Example 5 of the present invention.
[0034] In the figure: a, is the cytotoxicity determination of the material leachate; b, is the contact hemolysis rate determination of the material. DETAILED DESCRIPTION
[0035] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0036] In view of the problems of existing silicone dressings, the present invention provides a silicone moisturizing dressing. The preparation method of the silicone moisturizing dressing comprises the following steps:
[0037] S1: Prepare silica precursor.
[0038] S2: adding a pore-forming agent into the silica gel precursor, stirring the mixture evenly to obtain a silica gel mixture.
[0039] S3: Add the silicone mixture into the mold, heat and cure it, and take it out to obtain the initial product of the silicone dressing.
[0040] S4: After washing the initial silicone dressing product, perforation and / or surface hydrophilic modification are performed.
[0041] S6: After drying and sterilization, the medical silicone moisturizing dressing is obtained.
[0042] It is understandable that, in the present invention, the combination of the silica gel precursor and the pore-forming agent can first form micropores in the silica gel matrix, which is beneficial to the air permeability of the dressing. At the same time, during the hydrophilic modification, the modifier can treat the surface and interior of the silica gel.
[0043] It is understandable that the content of the pore-forming agent will affect the porosity and mechanical properties of the prepared dressing, and will also affect the liquid absorption rate. Properly increasing the amount of the pore-forming agent can simultaneously achieve an increase in the stretching ratio and the liquid absorption rate.
[0044] In some embodiments, in step S3, the mold is made of polymethyl methacrylate, has a depth of 0.5 to 50 mm, a width of 1 mm to 1000 mm, and a length of 1 mm to 1000 mm.
[0045] It can be understood that the porous network structure obtained by the present invention through drilling, using the micropores formed by the pore-forming agent and the holes obtained by drilling, has good tissue adhesion, can closely fit the irregular wound surface, absorb exudate and keep the wound base moist, and the excess exudate can be discharged from the micropores to the dressing surface, evaporated naturally or absorbed by the external dressing. However, the size of the pore spacing has an important influence on its mechanical properties, liquid absorption rate, and swelling rate.
[0046] Preferably, the present invention limits the parameters of the punching and performs surface modification after the punching, so as to achieve simultaneous surface modification of the pores obtained by the punching and the micropores obtained by the pore-forming agent, thereby improving the hydrophilicity of the entire silica gel while ensuring the basic mechanical properties of the silica gel, thereby improving the moisturizing performance.
[0047] The porosity of the silica gel dressing of the present invention is 30-75%.
[0048] The present invention will be further described below by way of examples and the like.
[0049] Example 1
[0050] A medical silicone moisturizing dressing, the preparation method of which comprises the following steps:
[0051] Step 1: 30 parts by mass of silica gel A and 30 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., the raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0052] Step 2: Add 40 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0053] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes;
[0054] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it;
[0055] Step 5: After drying the silicone dressing in an oven, sterilize it by irradiation and package it.
[0056] Example 2
[0057] A medical silicone moisturizing dressing, the preparation method of which comprises the following steps:
[0058] Step 1: 20 parts by mass of silica gel A and 20 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., the raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0059] Step 2: Add 60 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0060] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes;
[0061] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it;
[0062] Step 5: After drying the silicone dressing in an oven, sterilize it by irradiation and package it.
[0063] Example 3
[0064] A medical silicone moisturizing dressing, the preparation method of which is the same as that of Example 2, except that a punching process is added, and the specific method is as follows:
[0065] Step 1: 20 parts by mass of silica gel A and 20 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., the raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0066] Step 2: Add 60 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0067] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes;
[0068] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it;
[0069] Step 5: The obtained product is mechanically punched with a drill bit, with a hole diameter of 1 mm and a hole spacing of 10 mm;
[0070] Step 6: After punching, irradiation sterilization and packaging are carried out.
[0071] The schematic diagram of the structure and the schematic diagram of the cross-sectional structure of the silicone moisturizing dressing obtained in this embodiment are as follows: Figure 1-2 shown.
[0072] Example 4
[0073] A medical silicone moisturizing dressing, the preparation method of which is the same as that of Example 3, except that the hole spacing is reduced. The specific method is as follows:
[0074] Step 1: 20 parts by mass of silica gel A and 20 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., the raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0075] Step 2: Add 60 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0076] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes;
[0077] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it;
[0078] Step 5: The obtained product is mechanically punched with a drill bit, with a hole diameter of 1 mm and a hole spacing of 5 mm;
[0079] Step 6: After punching, irradiation sterilization and packaging are carried out.
[0080] Example 5
[0081] A medical silicone moisturizing dressing, the preparation method of which is the same as that of Example 2, except that a single-sided plasma treatment is performed after step 4, and no holes are punched. The specific method is as follows:
[0082] Step 1: 20 parts by mass of silica gel A and 20 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., the raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0083] Step 2: Add 60 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0084] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes;
[0085] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it;
[0086] Step 5: subject the obtained product to single-sided plasma treatment, and then spray 6wt% PVA solution on the surface, and spray the entire surface once; wherein, the conditions of plasma treatment are power 800W, distance 10mm, and time 20s.
[0087] Step 6: Dry the silicone dressing in an oven, sterilize it by irradiation and package it.
[0088] The schematic diagram of the structure and the schematic diagram of the cross-sectional structure of the silicone moisturizing dressing obtained in this embodiment are shown in FIG. Figure 3-4 shown. Figure 5 This is a scanning electron microscope image of the surface of the silicone dressing of this example, in which a large number of interconnected pores can be seen, indicating that the material has excellent liquid absorption potential.
[0089] Example 6
[0090] A medical silicone moisturizing dressing, in which perforation and hydrophilic modification are simultaneously used in preparation, the perforation conditions are the same as those in Example 3, and the hydrophilic modification conditions are the same as those in Example 5. The specific method is as follows:
[0091] Step 1: 20 parts by mass of silica gel A and 20 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., the raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0092] Step 2: Add 60 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0093] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes;
[0094] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it;
[0095] Step 5: The obtained product is mechanically punched with a drill bit, with a hole diameter of 1 mm and a hole spacing of 10 mm;
[0096] Step 6: subject the obtained product to single-sided plasma treatment, and then spray 6wt% PVA solution on the surface, and spray the entire surface once; wherein, the conditions of plasma treatment are power 800W, distance 10mm, and time 20s.
[0097] Step 7: After drying the silicone dressing in an oven, sterilize it by irradiation and package it.
[0098] Example 7
[0099] A medical silicone moisturizing dressing, the specific method is as follows:
[0100] Step 1: 16 parts by mass of silica gel A and 20 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0101] Step 2: Add 36 parts by weight of sodium chloride particles to the mixture prepared in step 1 and stir evenly;
[0102] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 40℃ oven for 10 minutes;
[0103] Step 4: Remove the cured silicone material from the mold, rinse it repeatedly in 30°C hot water to completely remove the sodium chloride particles and dry it;
[0104] Step 5: The obtained product is mechanically punched with a drill bit, with a hole diameter of 0.01 mm and a hole spacing of 0.05 mm;
[0105] Step 6: subject the obtained product to single-sided plasma treatment, and then spray 1wt% PVA solution on the surface, and spray the entire surface once; wherein, the conditions of plasma treatment are power of 500W, distance of 5mm, and time of 10s.
[0106] Step 7: After drying the silicone dressing in an oven, sterilize it by irradiation and package it.
[0107] Example 8
[0108] A medical silicone moisturizing dressing, the specific method is as follows:
[0109] Step 1: 30 parts by mass of silica gel A and 20 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor; wherein the raw materials of the silica gel precursor, i.e., the raw materials containing silica gel A and silica gel B, are purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
[0110] Step 2: Add 60 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0111] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with the mixed silicone stand for 5 minutes, then heat it in an 80℃ oven for 60 minutes;
[0112] Step 4: De-mold the cured silicone material, rinse it repeatedly in 90°C hot water to completely remove the sodium chloride particles and dry it;
[0113] Step 5: The obtained product is mechanically punched with a drill bit, with a hole diameter of 10 mm and a hole spacing of 5 mm;
[0114] Step 6: subject the obtained product to single-sided plasma treatment, and then spray 10wt% PVA solution on the surface, and spray the entire surface once; wherein, the conditions of plasma treatment are power of 1000W, distance of 15mm, and time of 30s.
[0115] Step 7: After drying the silicone dressing in an oven, sterilize it by irradiation and package it.
[0116] Comparative Example 1
[0117] A silicone dressing, the preparation method of which is as follows:
[0118] Step 1: 40 parts by mass of silica gel A and 40 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor;
[0119] Step 2: Add 20 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0120] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes;
[0121] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it;
[0122] In this comparative example, the surface of the silica gel material in step four is intact without holes, and the sodium chloride particles are completely wrapped and cannot be washed out, so the preparation steps cannot be completed to form a sample.
[0123] Comparative Example 2
[0124] A silicone dressing, the preparation method of which is as follows:
[0125] Step 1: 10 parts by mass of silica gel A and 10 parts by mass of silica gel B are fully mixed and stirred to prepare a silica gel precursor;
[0126] Step 2: Add 80 parts by weight of sodium chloride particles to the mixture obtained in step 1 and stir evenly;
[0127] Step 3: Pour the mixed raw materials into the mold so that the mixed materials evenly fill the entire mold. Let the mold with mixed silicone stand for 5 minutes, then heat it in a 60℃ oven for 20 minutes.
[0128] Step 4: De-mold the cured silicone material, rinse it repeatedly in 60°C hot water to completely remove the sodium chloride particles and dry it.
[0129] In this comparative example, after the sodium chloride particles were eluted from the silica gel material in step 4, the integrity was poor and could not be formed, and the preparation steps could not be completed to form a sample.
[0130] Test example:
[0131] The maximum stretching ratio of the silicone dressing prepared in the example was measured by an electronic universal testing machine (Changzhou Sanfeng Instrument Technology Co., Ltd.). The test results are shown in Table 1, where the maximum stretching ratio is equal to 183%.
[0132] Similarly, the maximum bearing capacity of the silicone dressing prepared in the embodiment is tested by an electronic universal testing machine, and the calculation formula is tensile strength (Mpa) = maximum force (N) / cross-sectional area (mm 2 ), and the results are shown in Table 1.
[0133] The silicone dressing prepared in the embodiment was placed in pure water to measure its swelling and calculate the swelling rate. The swelling rate was calculated by the formula: swelling rate (%) = ((G2-G1) / G1) × 100%, wherein G1 is the dry mass of the sample, and G2 is the mass of the sample after swelling and removal of free water. The results are shown in Table 1.
[0134] The silicone dressings prepared in the examples and comparative examples were placed in pure water to determine their liquid absorption and to calculate the liquid absorption rate. The liquid absorption rate was calculated as follows: liquid absorption rate (%) = ((Ms-Md) / Md) × 100%, wherein Ms is the total mass after absorbing water for a certain period of time, and Md is the mass of the dry sample. The results are shown in Table 1.
[0135] Table 1 shows the physical properties of the medical silicone moisturizing dressing prepared in the embodiment of the present invention.
[0136]
[0137] As can be seen from Table 1, the present invention optimizes the performance of silicone dressing by adjusting the proportion of pore-forming agent. By comparing Example 1 with Example 2, it can be seen that the proportion of pore-forming agent increases, the maximum stretching ratio and liquid absorption rate increase, but the maximum tensile strength is slightly weakened. In addition, by comparing Example 2 with Example 3 and Example 5, it can be seen that both punching and hydrophilic modification can increase the liquid absorption rate of the material, but the later punching operation reduces the mechanical strength of the material and reduces the tensile strength. In Example 4, after the hole spacing is reduced, its mechanical properties and liquid absorption rate are lower than those of Example 3. Example 6 significantly improves the swelling rate and liquid absorption rate on the basis of ensuring basic mechanical properties.
[0138] Safety Testing:
[0139] The cytotoxicity of the silica gel material in Example 5 was evaluated using the CCK8 kit. The silica gel prepared in Example 5 was 2 / 10ml concentration is placed in complete culture medium, incubated in a shaker at 37℃ for 24h, and the extract is prepared. 200μL 2k / well cells are inoculated on a 96-well plate and cultured for 8 hours at 37℃, 5% CO2, and 90% humidity. After adhesion, the extract and new culture medium are replaced, 200μL per well. After incubation for 24h, 10μL CCK-8 reagent is added to each well and incubated for 2 hours. The absorbance of the sample at 450nm is measured using an enzyme reader. The experimental group used the extract of the dressing and added the cck-8 reagent, the control group used the complete culture medium and added the cck-8 reagent, and the blank control group only used the complete culture medium. The calculation formula for cell viability is as follows:
[0140] Cell viability (%) = (OD 样品 -OD 空白 ) / (OD 对照 -OD 空白 ))×100%
[0141] For the hemolysis test, concentrated red blood cells were obtained by centrifuging fresh anticoagulated mouse whole blood at 2000 rpm for 10 minutes. The obtained red blood cells were washed several times with PBS until the supernatant became colorless and transparent. The purified red blood cells were further diluted with PBS to a final concentration of 5% (v / v). 300 μL of red blood cell suspension and 1 cm2 of silica gel material were added to 1 ml of PBS. Pure water and PBS were used as positive and negative controls, respectively. After incubation at 37°C for 2 hours, all samples were centrifuged at 2000 rpm for 5 minutes, and the absorbance of the supernatant was measured at 540 nm using a microplate reader. The hemolysis rate was calculated as follows:
[0142] Hemolysis rate (%) = ((OD 样品 -OD 阴性 ) / (OD 阳性 -OD 阴性 ))×100%
[0143] Conduct safety testing, the results are as follows Figure 6 The experimental results can prove that the silicone moisturizing dressing prepared by the present invention is safe and non-toxic.
[0144] The above is only a preferred embodiment of the present invention, and the present invention is not limited to the above embodiments. It is understood that other improvements and changes directly derived or associated by those skilled in the art without departing from the spirit and concept of the present invention should be considered to be included in the protection scope of the present invention.
Claims
1. A method for preparing a medical silicone moisturizing dressing, It is characterized in that The preparation method comprises the following steps: S1: Preparation of silica precursor; S2: adding a pore-forming agent to the silica gel precursor and stirring the mixture to obtain a silica gel mixture; S3: adding the silicone mixture into the mold, heating and curing, and taking it out to obtain the initial product of the silicone dressing; S4: washing the initial product of the silicone dressing, and then performing pore punching and / or surface hydrophilic modification; S5: After drying and sterilization, the medical silicone moisturizing dressing is obtained.
2. The preparation method according to claim 1, It is characterized in that In step S1, the raw material of the silica gel precursor is purchased from Shenzhen Guoyuan Technology Co., Ltd., model T00.
3. The preparation method according to claim 2, It is characterized in that The silica gel precursor comprises silica gel component A and silica gel component B. When used, silica gel component A and silica gel component B are mixed to obtain a silica gel precursor; wherein, The mass ratio of the silica gel component A to the silica gel component B is 0.8-1.5:
1.
4. The preparation method according to claim 1, It is characterized in that In step S2, the pore-forming agent includes any one of potassium nitrate, ammonium sulfate, ammonium chloride, sodium chloride, potassium chloride, and sucrose particles; and the mass ratio of the pore-forming agent to the silica gel precursor is 1:1 to 3:
2.
5. The preparation method according to claim 1, It is characterized in that In step S3, the material of the mold is polymethyl methacrylate; the temperature of the heating and curing is 10 to 100° C., and the time is 0.5 to 10 hours.
6. The preparation method according to claim 1, It is characterized in that In step S4, the washing temperature is 1 to 100° C. and the washing time is 0.5 to 10 hours.
7. The preparation method according to claim 1, It is characterized in that In step S4, the punching is to punch holes on the surface of the washed silica gel primary product; the punching method includes one of mechanical punching and laser punching; The hole diameter of the punched holes is 0.01 to 10 mm, and the distance between adjacent holes is 0.01 to 10 mm; The shape of the hole includes any one of a cylinder, a cone, and an irregular shape.
8. The preparation method according to claim 1, It is characterized in that In step S4, the hydrophilic modification is performed by soaking in dopamine hydrochloride, or spraying polyvinyl alcohol or carboxymethyl cellulose after plasma surface treatment.
9. The preparation method according to claim 8, It is characterized in that The concentration of dopamine hydrochloride is 0.1-0.5wt%; the immersion time is 12-48h; the concentration of polyvinyl alcohol is 1-10wt%; the power of the plasma surface treatment is 500-1000W, the distance is 5-15mm, and the time is 10-30s.
10. A medical silicone moisturizing dressing prepared by the preparation method according to any one of claims 1 to 9.