Hydrophilic surface molecularly imprinted chitosan microspheres as well as preparation method and application thereof
Hydrophilic surface molecular imprint chitosan microspheres prepared by surface molecular imprinting technology solve the problems of poor water phase recognition ability and small adsorption capacity of existing hydrophilic blotting materials, achieving efficient water phase recognition and adsorption effects. And avoid the use of toxic chemical reagents during the preparation process, providing a green and environmentally friendly solution.
Patent Information
- Application Number
- CN202411063509.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The existing hydrophilic blotting materials have poor water phase recognition ability, small adsorption capacity, slow mass transfer rate, and the use of toxic and harmful chemical reagents during preparation.
The hydrophilic surface molecular imprinted chitosan microspheres were prepared by surface molecular imprinting technology. By mixing the virtual template with chitosan solution, sedimenting to the surface of glucose carbon balls, and removing the template with ultrasonic acid using sulfuric acid solution, a good dispersion was prepared. Sexual and highly hydrophilic microspheres.
It realizes an adsorbent material with efficient water phase recognition ability, strong specific recognition ability, large adsorption capacity and fast mass transfer rate. It is suitable for the extraction and separation of complex samples, and the preparation process is green and environmentally friendly, avoiding the use of toxic chemical reagents.
Smart Images

Figure HDA0004978688790000011 
Figure HDA0004978688790000012 
Figure HDA0004978688790000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of molecular imprinting technology and sample pretreatment, in particular to a hydrophilic surface molecular imprinting chitosan microsphere, a preparation method and application thereof. Background Art
[0002] The main purpose of sample pretreatment is to reduce the interference of coexisting components in the sample on the detection, remove components in the sample that are unfavorable to the instrument, extend the life of the instrument, and at the same time enrich and concentrate the target, increase the response value of the component to be tested to improve the sensitivity of the detection. Among the many sample pretreatment methods, solid phase extraction is one of the most commonly used sample pretreatment methods, and its core is the selection and preparation of adsorbents. At present, the common adsorbents on the market are C 18 , HLB, silica gel, porous resin, etc., but the above adsorbents have a single adsorption force and lack selectivity for specific targets in complex systems. Therefore, the development of highly selective adsorbents is of great significance for improving the extraction and separation of trace targets in complex samples.
[0003] Compared with natural enzymes, antigens and antibodies and other biorecognition systems, molecular imprinting materials are simple to prepare, inexpensive, and have higher mechanical strength and acid and alkali resistance. They can be used in more complex and harsh environments, effectively overcoming the problem of low extraction efficiency of biorecognition systems in complex matrices. Molecular imprinting materials have been widely used in environmental monitoring, food safety, and early disease diagnosis due to their excellent selectivity, structural predetermination, and practicality. However, the recognition of targets by traditional molecular imprinting materials is mostly limited to organic solvent systems, and the recognition ability is poor in polar systems such as water. In addition, traditional molecular imprinting materials are mostly prepared by bulk polymerization and other methods. The imprinting sites are easy to embed, the mass transfer rate is slow, and the extraction efficiency of trace components in complex systems is low.
[0004] In order to solve the problem of poor water phase recognition ability of molecular imprinting materials, Yan et al. combined molecular imprinting technology with the preparation process of hydrophilic resins to prepare a series of hydrophilic molecular imprinting materials, realizing the specific extraction and separation of trace components (pesticides, persistent organic pollutants, tumor markers, etc.) in complex samples such as environmental water, food and urine samples (Analytical Chemistry, 2015, 87 (21): 11084-11091; Green Chemistry, 2024, 26 (4): 2000-2010). In Chinese invention patent CN202110273357.7, amino-functionalized magnetic graphene oxide was used as the substrate, formaldehyde was used as the hydrophilic cross-linking agent, and resorcinol and melamine were used as double hydrophilic monomers. Surface imprinting technology was used to prepare magnetic graphene oxide hydrophilic molecular imprinting nanocomposite resins, which realized the separation and detection of trace chlorophenol pollutants in environmental water. These hydrophilic imprinted resin materials mostly use toxic and harmful chemical reagents in the preparation process, which seriously endangers human health and does not conform to the green chemistry principles advocated now. Therefore, the development of green hydrophilic imprinted materials with rapid target recognition is a hot issue to be solved in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a hydrophilic surface molecular imprinted chitosan microsphere, a preparation method and application thereof, so as to solve the problems that the imprinting sites of the existing hydrophilic imprinted polymer are not fully utilized, the mass transfer rate is slow, the adsorption capacity per unit mass of the adsorbent is low, and the preparation process uses toxic and harmful chemical reagents that are easy to cause harm to human health.
[0006] The present invention is achieved in that:
[0007] The invention discloses a hydrophilic surface molecular imprinted chitosan microsphere, which is prepared by mixing a virtual template with a chitosan solution, adding a sodium hydroxide solution to precipitate the chitosan containing the virtual template onto the surface of a glucose carbon sphere, then using a sulfuric acid solution for ultrasonic acid hydrolysis, and finally removing the virtual template.
[0008] Preferably, the virtual template is naphthylethylenediamine hydrochloride; the chitosan solution is obtained by dissolving chitosan in an acetic acid aqueous solution with a volume fraction of 0.5 to 5.0%; the sodium hydroxide solution is an aqueous solution of sodium hydroxide with a concentration of 0.1 to 10.0 mol / L; the glucose carbon spheres are brown-red solid powders obtained by polymerizing a glucose aqueous solution with a concentration of 0.01 to 10.0 g / mL in a hydrothermal reactor; and the sulfuric acid solution is an aqueous sulfuric acid solution with a concentration of 0.1 to 5.0 mol / L.
[0009] The hydrophilic surface molecularly imprinted chitosan microspheres prepared by the invention are in a micrometer-level spherical structure with uniform size, have good dispersibility, have a large number of hydrophilic functional groups on the surface, and have excellent hydrophilicity.
[0010] Preferably, the chitosan is any one of high molecular weight chitosan, medium molecular weight chitosan and low molecular weight chitosan.
[0011] Preferably, the chitosan solution is formed by adding 0.013-7.28 g of chitosan to 20 mL of acetic acid aqueous solution; and the amount of the virtual template is 0.01-10.0 mmol.
[0012] Preferably, the ultrasonic acid hydrolysis has an ultrasonic input power of 10 to 200 W and a time of 1 to 300 min.
[0013] Preferably, when preparing glucose carbon spheres, the concentration of glucose is 0.01 to 10.0 g / mL, the heating temperature is 80 to 180° C., and the heating time is 2 to 48 h.
[0014] The eluent used to wash away the template can be a common eluent, such as at least one of methanol, acetonitrile, acetone, methanol-acetic acid, acetonitrile-acetic acid, acetone-acetic acid, etc.
[0015] Preferably, after the template is washed away, the obtained solid is dried by vacuum drying or freeze drying at a vacuum drying temperature of 25 to 80°C.
[0016] The hydrophilic surface molecularly imprinted chitosan microspheres prepared by the present invention can be used as an adsorbent, and can also have corresponding uses in biosensing, simulated antibody, drug delivery or biomimetic catalysis and the like.
[0017] As adsorbents, hydrophilic surface molecularly imprinted chitosan microspheres can specifically identify tumor markers in human urine, naphthalene plant hormones in traditional Chinese medicine, and indole plant hormones, and can be well applied in environmental monitoring, food safety, and early diagnosis of diseases.
[0018] Preferably, the tumor markers in human urine include but are not limited to 5-hydroxyindoleacetic acid (5-HIAA) and 5-hydroxytryptamine (5-HT); the naphthalene plant hormones and indole plant hormones in the traditional Chinese medicine include but are not limited to 1-naphthaleneacetic acid (NAA), 2-naphthaleneoxyacetic acid (BNOA), naphthylacetamide (NAD), 3-indoleacetic acid (IAA), indolepropionic acid (IPA), and 3-indolebutyric acid (IBA).
[0019] The present invention adopts surface molecular imprinting technology to prepare hydrophilic surface molecular imprinting chitosan microspheres. The obtained hydrophilic surface molecular imprinting chitosan microspheres have large adsorption capacity, fast mass transfer rate, strong specific recognition ability, high extraction efficiency, and excellent water phase recognition ability. They can be used as adsorbent materials for solid phase extraction and applied to the specific extraction and separation of multiple types of targets in complex sample matrices, making up for the shortcomings of existing molecular imprinting materials such as weak water phase recognition ability, low selectivity, small adsorption capacity and slow mass transfer rate. They have broad application prospects in the fields of environmental management, chromatographic separation, food safety, etc.
[0020] The preparation method of the invention is simple and low in cost. In the process of preparing the hydrophilic surface molecular imprinted chitosan microspheres, the use of toxic chemical reagents is avoided, the consumption of organic reagents is reduced, the invention is green and environmentally friendly, is friendly to human health and the environment, and has the potential for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The figures are scanning electron microscope (SEM) characterization images of the materials obtained in Example 1 and Comparative Example 1. Among them, (A) is the SEM image of the carbon sphere (CS) obtained in Example 1, (B) is the SEM image of the hydrophilic surface molecularly imprinted chitosan microsphere (CMIP) obtained in Example 1, and (C) is the SEM image of the non-imprinted chitosan microsphere material (NIP) obtained in Comparative Example 1.
[0022] Figure 2 It is the Fourier transform infrared spectra of the carbon sphere (CS) obtained in Example 1, the hydrophilic surface molecularly imprinted chitosan microsphere (CMIP) and the non-imprinted chitosan microsphere material (NIP) obtained in Comparative Example 1.
[0023] Figure 3 This is a graph showing the adsorption of 5-hydroxyindoleacetic acid (5-HIAA) when the materials obtained in Example 1 and Comparative Example 1 are used as adsorbents.
[0024] Figure 4 It is a comparison chart of the adsorption amount of 1-naphthylacetic acid (NAA), 2-naphthyoxyacetic acid (BNOA), and 3-indolebutyric acid (IBA) when the materials obtained in Example 1 and Comparative Example 1 are used as adsorbents.
[0025] Figure 5 This is a comparison chart of the adsorption amounts of 5-HIAA, vanillylmandelic acid, thiamphenicol, homovanillic acid, tetracycline hydrochloride, and florfenicol when the materials obtained in Example 1 and Comparative Example 1 are used as adsorbents.
[0026] Figure 6 This is a comparison chart of the adsorption amounts of NAA, BNOA, IBA, sodium p-chlorophenoxyacetate, terbuthylazine and gibberellin when the materials obtained in Example 1 and Comparative Example 1 are used as adsorbents.
[0027] Figure 7 This is the separation chromatogram of the CMIP synthesized in Example 1 used to detect 5-HIAA in urine.
[0028] Figure 8 The extraction recovery rates of 5-HIAA in spiked urine samples were compared using CMIP and CS synthesized in Example 1 of the present invention, NIP prepared in Comparative Example 1, and commercial adsorbent materials.
[0029] Fig. 9 The extraction recovery rates of NAA, BNOA and IBA in tangerine peel samples by CMIP and CS synthesized in Example 1 of the present invention, the NIP material prepared in Comparative Example 1 and commercial adsorbent materials are compared. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with the examples. The following examples are for illustration only. The processes and methods not described in detail in the following examples are conventional methods known in the art. The reagents used in the examples are all analytically pure or chemically pure, and can be commercially available or prepared by methods well known to those of ordinary skill in the art. The described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] Using naphthylethylenediamine hydrochloride as a virtual template molecule, the following method was used to synthesize hydrophilic surface molecularly imprinted chitosan microspheres CMIP:
[0033] (1) Weigh 7.2 g of glucose, add 100 mL of deionized water, stir evenly at room temperature until completely dissolved, transfer the glucose solution to a 200 mL polytetrafluoroethylene-lined stainless steel reactor, and heat at 180°C for 10 h. After cooling to room temperature, high-speed centrifugation was performed to obtain a brown-red solid, which was washed several times with deionized water and 95% medical alcohol, washed with deionized water until neutral, and freeze-dried to obtain glucose carbon spheres (CS).
[0034] (2) Weigh 0.1 g of glucose carbon spheres and place them in a 100 mL round-bottom flask. Add 20 mL of 1.0% acetic acid aqueous solution and sonicate for 2 h to evenly disperse the carbon spheres in the acetic acid aqueous solution. Then add 0.078 g of low molecular weight chitosan (purchased from Sigma-Aldrich) and stir at room temperature at 500 rpm for 6 h.
[0035] (3) 1.5 mmol virtual template naphthylethylenediamine hydrochloride was added to the round-bottom flask of step (2), and stirred at room temperature and 500 rpm for 24 h. Then, 25 mL of 1 mol / L sodium hydroxide solution was added to the round-bottom flask, and stirred at room temperature and 500 rpm for 3 h. After that, the supernatant was removed by high-speed centrifugation to obtain a brown solid, which was washed several times with deionized water.
[0036] (4) 10 mL of 0.5 mol / L sulfuric acid solution was added to the brown solid, and ultrasonic dispersion was performed at a power of 150 W for 30 min. Methanol-acetic acid (9:1, v / v) was added to clean the template. After the template was completely removed, it was washed with deionized water until neutral, and then freeze-dried to obtain hydrophilic surface molecularly imprinted chitosan microspheres CMIP.
[0037] Comparative Example 1
[0038] Non-imprinted chitosan microspheres were synthesized using the following method:
[0039] (1) Weigh 7.2 g of glucose, add 100 mL of deionized water, stir evenly at room temperature until completely dissolved, transfer the glucose solution to a 200 mL polytetrafluoroethylene-lined stainless steel reactor, and heat at 180°C for 10 h. After cooling to room temperature, high-speed centrifugation was performed to obtain a brown-red solid, which was washed several times with deionized water and 95% medical alcohol, washed with deionized water until neutral, and freeze-dried to obtain glucose carbon spheres.
[0040] (2) Weigh 0.1 g of glucose carbon spheres and place them in a 100 mL round-bottom flask. Add 20 mL of 1.0% acetic acid aqueous solution and sonicate for 2 h to evenly disperse the carbon spheres in the acetic acid aqueous solution. Then add 0.078 g of low molecular weight chitosan (purchased from Sigma-Aldrich) and stir at room temperature at 500 rpm for 6 h.
[0041] (3) 25 mL of 1 mol / L sodium hydroxide solution was added to a round-bottom flask, and the mixture was stirred at room temperature and 500 rpm for 3 h. The supernatant was then removed by high-speed centrifugation to obtain a brown solid, which was then washed several times with deionized water.
[0042] (4) 10 mL of 0.5 mol / L sulfuric acid solution was added to the brown solid, and ultrasonic dispersion was performed at a power of 150 W for 30 min. Methanol was added to wash the reaction intermediate and unreacted raw materials. After washing with deionized water until neutral, the solid was freeze-dried to obtain non-imprinted chitosan microspheres NIP.
[0043] The hydrophilic surface molecularly imprinted chitosan microspheres obtained in Example 1 and the non-imprinted chitosan microspheres obtained in Comparative Example 1 were characterized by SEM and Fourier transform infrared spectroscopy, respectively. The results are shown in FIG. Figures 1-2shown.
[0044] from Figure 1 It can be seen that the electron microscope images of hydrophilic surface molecularly imprinted chitosan microspheres CMIP and non-imprinted chitosan microspheres NIP are similar. The overall structure is loose and porous, and they are spherical particles with no significant difference in appearance. The particle size of a single microsphere is about 0.4 μm.
[0045] from Figure 2 It can be seen that the infrared spectra of CMIP and NIP are similar, indicating that the types of functional groups on the surfaces of the two prepared chitosan microsphere materials are basically the same. -1 The broad peak at 1704 cm -1 and 1619cm -1 The absorption peaks at 1630 cm are the stretching vibration peaks of C=O and C=C on the surface of carbon spheres. -1 and 1154cm -1 The absorption peaks at are characteristic peaks of chitosan, which are the bending vibration peak of -NH2 and the stretching vibration peak of CN, indicating that chitosan is successfully deposited on the surface of carbon spheres. In addition, the infrared spectrum results show that the surface of chitosan microspheres has abundant hydrophilic groups, which makes it have good hydrophilicity.
[0046] The hydrophilic chitosan microspheres obtained in Example 1 and Comparative Example 1 were used as adsorbents to investigate their adsorption performance. 3.0 mg of the dried hydrophilic surface molecularly imprinted chitosan microspheres CMIP and non-imprinted hydrophilic chitosan microspheres NIP were accurately weighed and placed in a 10 mL centrifuge tube. 2.0 mL of a 100 μg / mL standard aqueous solution containing 5-hydroxyindoleacetic acid (5-HIAA) was added, and the mixture was shaken at 25°C for 12 h, and then centrifuged at 4000 rpm for 3 min. The supernatant was passed through a membrane (0.22 μm) and analyzed by HPLC-UV. The results are shown in FIG. Figure 3 As shown. Figure 3 It can be seen that the adsorption of hydrophilic surface molecularly imprinted chitosan microspheres CMIP as adsorbent is better than that of non-imprinted chitosan microspheres NIP.
[0047] The hydrophilic chitosan microspheres obtained in Example 1 and Comparative Example 1 were used as adsorbents to investigate their adsorption performance. 3.0 mg of dried hydrophilic surface molecularly imprinted chitosan microspheres CMIP and non-imprinted chitosan microspheres NIP were accurately weighed and placed in a 10 mL centrifuge tube. 2.0 mL of a 100 μg / mL standard aqueous solution containing 1-naphthylacetic acid (NAA), 2-naphthyoxyacetic acid (BNOA), and 3-indolebutyric acid (IBA) was added. The mixture was shaken at 25°C for 12 hours, and then centrifuged at 4000 rpm for 3 minutes. The supernatant was passed through a membrane (0.22 μm) and analyzed by HPLC-UV. The results are shown in FIG. Figure 4As shown. Figure 4 It can be seen that the adsorption of hydrophilic surface molecularly imprinted chitosan microspheres CMIP as adsorbent is better than that of non-imprinted chitosan microspheres NIP.
[0048] The hydrophilic surface molecularly imprinted chitosan microspheres CMIP prepared in Example 1 were subjected to competitive adsorption experiments to detect their specific recognition ability.
[0049] Competitive adsorption study of CMIP: Accurately weigh 3.0 mg of CMIP prepared in Example 1 and NIP prepared in Comparative Example 1 and place them in different 10 mL centrifuge tubes. Add 2.0 mL of mixed standard solution to the centrifuge tubes. The mixed standard solution is a mixture of 5-HIAA, vanillylmandelic acid, thiamphenicol, homovanillic acid, tetracycline hydrochloride, and florfenicol standard solutions. The standard solutions of 5-HIAA, vanillylmandelic acid, thiamphenicol, homovanillic acid, tetracycline hydrochloride, and florfenicol are all standard solutions with a concentration of 100 μg / mL. Set up 3 centrifuge tubes in 3 parallel groups. Place the centrifuge tubes in a constant temperature oscillator at 25°C and 300 rpm for 12 hours. After adsorption is completed, centrifuge at 4000 rpm, take the supernatant, filter it with a 0.22 μm filter membrane (nylon 66), and then detect it by HPLC. The results are as follows Figure 5 shown.
[0050] Figure 5 In the formula, 1 represents 5-HIAA, 2 represents vanillylmandelic acid, 3 represents thiamphenicol, 4 represents homovanillic acid, 5 represents tetracycline hydrochloride, and 6 represents florfenicol. Figure 5 It can be seen that the adsorption performance of CMIP for 5-HIAA is much greater than that of vanillylmandelic acid, thiamphenicol, homovanillic acid, tetracycline hydrochloride, and florfenicol. The imprinted pores of CMIP have a certain specific recognition ability for 5-HIAA, making its adsorption capacity for 5-HIAA much greater than that of other compounds.
[0051] Competitive adsorption of CMIP: 3.0 mg of CMIP prepared in Example 1 and NIP prepared in Comparative Example 1 were accurately weighed and placed in different 10 mL centrifuge tubes. 2.0 mL of NAA, BNOA, IBA, sodium p-chlorophenoxyacetate, terbuthylazine, and gibberellin mixed standard solutions (the concentration of each standard solution was 100 μg / mL) were added to the centrifuge tubes. Three parallel groups were placed in a constant temperature oscillator at 25°C and 300 rpm for 12 h. After adsorption was completed, the tubes were centrifuged at 4000 rpm, the supernatant was taken, filtered using a 0.22 μm filter membrane (nylon 66), and then tested by HPLC. The results are shown in Figure 2. Figure 6 shown.
[0052] Figure 6In the formula, 1 represents BNOA, 2 represents IBA, 3 represents NAA, 4 represents sodium p-chlorophenoxyacetate, 5 represents terbuthylazine, and 6 represents gibberellin. Figure 6 It can be seen that the adsorption performance of CMIP for NAA, BNOA and IBA is much greater than that for sodium 4-chlorophenoxyacetate, terbuthylazine and gibberellin. The imprinted pores of CMIP have a certain specific recognition ability for 1-naphthylacetic acid, 2-naphthylacetic acid and 3-indolebutyric acid, making its adsorption capacity for NAA, BNOA and IBA much greater than that for other competitive molecules.
[0053] The hydrophilic surface molecularly imprinted chitosan microspheres CMIP prepared in Example 1 were applied to the specific detection of 5-hydroxyindoleacetic acid (5-HIAA) in urine.
[0054] Urine samples were obtained from six healthy volunteers (2 females and 4 males). After repeated freezing and thawing, the urine samples were centrifuged at 10,000 rpm for 5 min and filtered using a 0.22 μm filter membrane (nylon 66). 5.0 mL of urine was diluted to 50.0 mL with deionized water and 0.1 mol L -1 The pH of urine was adjusted to 4.0 with hydrochloric acid.
[0055] First, accurately weigh 15.0 mg of CMIP material and place it in a 3.0 mL SPE column, with a frit plate placed above and below. Use 1.0 mL of methanol and 1.0 mL of water to activate the material, load 1.0 mL of urine sample, use 0.4 mL of water to elute impurities, and finally add 1.0 mL of methanol-acetic acid (9:1, v / v) to elute, collect the eluate, evaporate it with nitrogen, and re-dissolve it with 0.5 mL of mobile phase. Detect by HPLC, the chromatographic conditions are: Acclaim TM 120C-18 (250mm×4.6mm, 5μm) chromatographic column (Thermo Fisher Scientific, USA). Mobile phase: acetonitrile-water (0.1% formic acid) (20:80, v / v), flow rate: 1.0mL / min, wavelength: 278nm, column oven: 25℃, injection volume 60μL. See the detection and separation chromatogram for details. Figure 7 .
[0056] Figure 7 In the figure, a is the chromatogram of the spiked urine sample without treatment, and b is the chromatogram of the spiked urine sample after SPE treatment. Figure 7 As can be seen in b, there is no interference near the peak time of the target, and there is no interfering chromatographic peak from other components in the urine sample, indicating that the established pretreatment method has good enrichment and purification capabilities and can separate and detect trace 5-hydroxyindoleacetic acid (5-HIAA) from urine samples.
[0057] The CS and hydrophilic surface molecular imprinted chitosan microspheres CMIP prepared in Example 1 and the NIP prepared in Comparative Example 1 were compared with commercial adsorbents such as HLB, C18, WAX, and MCX, taking the recovery rate of 5-HIAA as an indicator. CMIP, CS, and NIP were extracted using the optimized optimal extraction conditions. Taking CMIP as an example, the optimized optimal extraction conditions are: weigh 15.0 mg CMIP and place it in a 3.0 mL SPE column, place a sieve plate on the top and bottom, and use 1.0 mL methanol and 1.0 mL water to activate the material; add 1.0 mL of urine sample with a pH of 4.0, rinse with 0.4 mL of water, add 1.0 mL of methanol-acetic acid (9:1, v / v) to elute, collect the eluate, evaporate with nitrogen, and use 0.5 mL of mobile phase to re-dissolve and analyze by injection. The commercial adsorbent was extracted using the method reported in existing literature (such as the following literature 1-4). The results are as follows Figure 8 As shown in the figure, 5-HIAA has the highest recovery rate when CMIP is used as the adsorbent. CMIP has unique imprinted pores, and has adsorption forces such as hydrogen bonding and π-π conjugation with 5-HIAA, which has stronger affinity and higher recovery rate.
[0058] The CMIP and CS prepared in Example 1 and the NIP prepared in Comparative Example 1 were compared with commercial adsorbents such as SAX, C18, HLB and MAX. The results are as follows: Fig. 9 As shown. CMIP, CS and NIP were extracted using the optimized best extraction conditions. Taking CMIP as an example, the optimized best extraction conditions are: 30 mg of CMIP was placed in a 3.0 mL SPE column, with a sieve plate placed on the top and bottom, and the material was activated with 1.0 mL of methanol and 1.0 mL of water; 1.0 mL of tangerine peel and white tea sample with a pH of 3 was added, rinsed with 0.5 mL of water, and eluted with 1.0 mL of acetonitrile-acetic acid (9:1, v / v), and the eluate was collected, evaporated with nitrogen, and re-dissolved with 0.5 mL of mobile phase and analyzed by injection. The commercial adsorbent was extracted using the method reported in existing literature (such as the following literature 5-8). By Fig. 9 It can be seen that when CMIP is used as an adsorbent, it has the highest recovery rate for NAA, BNOA, and IBA and is significantly better than commercial adsorbents. The reason is that CMIP has multiple forces such as hydrogen bonds and π-π conjugation with the three naphthalene plant hormones and indole plant hormones, and has a stronger affinity.
[0059] The above describes in detail the use of the hydrophilic surface molecularly imprinted chitosan microspheres prepared by the present invention as adsorbents. In addition, the hydrophilic surface molecularly imprinted chitosan microspheres in the present invention can also be used in biosensors, simulated antibodies, drug delivery or biomimetic catalysis.
[0060] Literature:
[0061] [1] Song Z, Cai M, Zhao Y, et al. Simultaneous determination of 14 biogenic amines and metabolites in bullfrog blood using UFLC-MS / MS with SPE[J]. Analytical Methods, 2015, 7(18): 7436 - 7442.
[0062] [2] Uutela P, Reinila R, Harju K, et al. Analysis of intact glucuronides and sulfates of serotonin, dopamine, and their phase I metabolites in rat brain microdialysates by liquid chromatography - tandem mass spectrometry[J]. Analytical Chemistry, 2009, 81(20): 8417 - 8425.
[0063] [3] Tohmola N, Itkonen O, Sane T, et al. Analytical and preanalytical validation of a new mass spectrometric serum 5 - hydroxyindoleacetic acid assay as neuroendocrine tumor marker[J]. Clinica Chimica Acta, 2014, 428: 38 - 43.
[0064] [4] Eugster P J, Dunand M, Grund B, et al. Quantification of serotonin and eight of its metabolites in plasma of healthy volunteers by mass spectrometry[J]. Clinica Chimica Acta, 2022, 535: 19 - 26.
[0065] [5]Tadeusz P,et al.Simultaneous Determination of Indolic Compounds inPlant Extracts by Solid-Phase Extraction and High-Performance LiquidChromatography with UV and Fluorescence Detection[J].Food Anal.Methods,2015,8:2169-2177.
[0066] [6]Zheng H,Gang L,et al.Aliquid chromatography tandem massspectrometry method for simultaneous determination of acid / alkalinephytohormones in grapes[J].Chromatography B,881-882(2012)83-89.
[0067] [7]P.I.Dobrev,et al.Purification and determination of plant hormonesauxin and abscisic acid using solid phase extraction and two-dimensional highperformance liquid chromatography[J].Chromatography A,1075(2005)159–166.
[0068] [8]Ming-L Ch,et al.Highly sensitive and quantitative profiling ofacidic phytohormones using derivatization approach coupled with nano-LC-ESI-Q-TOF-MS analysis[J].Chromatography B,905(2012)67-74。
Claims
1. A method for preparing hydrophilic surface molecularly imprinted chitosan microspheres, characterized in that: The virtual template and chitosan solution are mixed to form a virtual template-chitosan complex, and then sodium hydroxide solution is added to precipitate the virtual template-chitosan complex onto the surface of glucose carbon spheres. Then, sulfuric acid solution is used for ultrasonic acid hydrolysis, and finally the virtual template is removed to obtain hydrophilic surface molecularly imprinted chitosan microspheres. The virtual template is naphthylethylenediamine hydrochloride; the chitosan solution is obtained by dissolving chitosan in an acetic acid aqueous solution with a volume fraction of 0.5-5.0%; the glucose carbon spheres are brown-red solid powders obtained by polymerizing a glucose aqueous solution with a concentration of 0.01-10.0 g / mL in a hydrothermal reactor.
2. The method for preparing hydrophilic surface molecularly imprinted chitosan microspheres according to claim 1, characterized in that: The chitosan is any one of high molecular weight chitosan, medium molecular weight chitosan and low molecular weight chitosan.
3. The method for preparing hydrophilic surface molecularly imprinted chitosan microspheres according to claim 1, wherein: The chitosan solution is formed by adding 0.013-7.28 g of chitosan to 20 mL of acetic acid aqueous solution; the amount of the virtual template is 0.01-10.0 mmol.
4. The method for preparing hydrophilic surface molecularly imprinted chitosan microspheres according to claim 1, wherein: The ultrasonic acid hydrolysis has an ultrasonic input power of 10 to 200 W and a time of 1 to 300 minutes.
5. The method for preparing hydrophilic surface molecularly imprinted chitosan microspheres according to claim 1, wherein: The glucose carbon spheres are obtained by polymerizing a glucose aqueous solution with a concentration of 0.01 to 10.0 g / mL in a hydrothermal reactor at a heating temperature of 80 to 180° C. for a heating time of 2 to 48 hours.
6. The method for preparing hydrophilic surface molecularly imprinted chitosan microspheres according to claim 1, wherein: The sulfuric acid solution is a sulfuric acid aqueous solution with a concentration of 0.1 to 5.0 mol / L.
7. The method for preparing hydrophilic surface molecularly imprinted chitosan microspheres according to claim 1, wherein: The sodium hydroxide solution is a sodium hydroxide aqueous solution with a concentration of 0.1 to 10.0 mol / L.
8. Hydrophilic surface molecularly imprinted chitosan microspheres prepared by the method according to any one of claims 1 to 7.
9. Use of the hydrophilic surface molecularly imprinted chitosan microspheres according to claim 8 in adsorbents, biosensors, simulated antibodies, drug delivery or biomimetic catalysis.
10. The use according to claim 9, wherein the hydrophilic surface molecularly imprinted chitosan microspheres are used as an adsorbent in the detection of tumor markers, indole plant growth regulators, and naphthalene plant growth regulators in urine.
Citation Information
Patent Citations
Hydrophilic molecular imprinting nano-composite resin based on magnetic graphene oxide as well as preparation method and application of hydrophilic molecular imprinting nano composite resin
CN113004479A