Conductive composite frame
By using conductive composite frames of metal powder and thin wires in offshore photovoltaic modules, the problem of insufficient frame corrosion and conductivity in marine environments is solved, high conductivity and corrosion resistance are achieved, international electrical safety standards are met, and the problem of insufficient frame corrosion and conductivity in marine environments is improved. The security and reliability of the system.
Patent Information
- Application Number
- CN202411089121.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
AI Technical Summary
The aluminum frames and steel frames of offshore photovoltaic modules are easily corroded in the marine environment, causing the components to fail, and the composite frames cannot conduct electricity and cannot meet international electrical safety standards, increasing the risk of electric shock and fire.
Use conductive composite frames with a mass percentage of 5 to 10%, metal fine wires 5 to 10%, glass fiber 65 to 85%, and resin 15 to 35%, to ensure the material by mixing the metal powder and metal fine wires. The conductive properties and corrosion resistance are improved by molding and curing.
It achieves good conductivity and corrosion resistance without increasing cost and weight, meets the grounding requirements of the photovoltaic system, reduces electric shock and fire risks, and improves the safety and reliability of the system.
Smart Images

Figure CN118978803A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic assembly preparation, in particular to a conductive composite frame. Background Art
[0002] Offshore photovoltaic technology is derived from the expansion of land-based photovoltaic systems. It uses floating platforms to install photovoltaic modules on the sea surface and maintains stability through anchoring systems. Its main advantage is to make full use of the vast space and superior solar energy resources of the ocean, but it also faces challenges such as corrosion and maintenance difficulties. At present, offshore photovoltaic technology is developing rapidly in China, Europe, Japan and other places, gradually moving from pilot projects to large-scale commercial applications. In the future, it will rely on material innovation and standardization to promote further development.
[0003] At present, most photovoltaic modules use aluminum frames and steel frames, and seawater is highly corrosive and contains salt and other chemicals. Aluminum frames and steel frames are easily corroded in the marine environment, causing module failure and affecting the service life and reliability of the photovoltaic system. In contrast, composite frame modules can prevent the frame from being corroded by seawater. However, according to international requirements, photovoltaic modules need to be installed with ground wires, but composite frames cannot be installed with ground wires because they are not conductive. In the event of an electrical fault or lightning strike, they may not be able to effectively guide the current, increasing the risk of electric shock and fire, and failing to meet international electrical safety standards. Summary of the invention
[0004] The purpose of the present invention is to provide a conductive composite frame to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is a conductive composite frame, which comprises the following raw materials by mass percentage: 5-10% metal powder, 5-10% metal fine wire, 65-85% glass fiber and 15-35% resin.
[0007] Further, the metal powder includes copper powder, aluminum powder or nickel powder;
[0008] The metal thin wires include copper wires.
[0009] Furthermore, the resin includes polyurethane or epoxy acrylate.
[0010] Furthermore, the particle size of the metal powder is 1 to 10 microns; the diameter of the metal wire is 5 microns, and the aspect ratio is 50:1; the diameter of the glass fiber is 20 microns, and the length is the same as that of the conductive composite frame.
[0011] Metal powder has excellent electrical conductivity and corrosion resistance, good dispersibility and appropriate particle size, and can be evenly distributed in the composite material.
[0012] Mixing metal powder, metal fine wire, glass fiber and resin in the above proportions can not only maintain the mechanical strength and corrosion resistance of the material, but also ensure conductivity.
[0013] Adding metal powder and metal wire in the above proportions can achieve good conductivity without significantly increasing cost and weight.
[0014] Glass fiber can improve the mechanical strength and corrosion resistance of the composite frame.
[0015] The second technical solution of the present invention is a method for preparing the above-mentioned conductive composite frame, comprising the following steps:
[0016] The raw materials are mixed evenly to obtain a mixture, the mixture is molded and then cured to obtain the conductive composite frame.
[0017] Furthermore, the compression molding specifically includes: adding the mixed material into a mold preheated to 120°C, then applying a pressure of 20MPa (to ensure uniform distribution of the raw materials), maintaining for 10 to 20 minutes, then heating to 150°C (to ensure that the resin completely flows and fills the mold), and increasing the pressure to 50MPa at 150°C (to ensure that the raw materials are tightly combined and excess bubbles and voids are removed), and maintaining for 30 to 40 minutes.
[0018] Furthermore, the curing treatment is carried out at a temperature of 60 to 80° C. and for a time of 2 to 4 hours.
[0019] Furthermore, the mixing method is selected from any one of mechanical stirring, high shear mixing, solvent-assisted mixing, ultrasonic mixing or air flow stirring.
[0020] The conditions for high shear mixing are: shear speed of 3000-5000 rpm, mixing time of 15-30 min, and temperature maintained at 20-25°C.
[0021] The curing process ensures the mechanical strength and stability of the material while maintaining the metal's conductive properties.
[0022] The third technical solution of the present invention: an application of the above-mentioned conductive composite frame in the photovoltaic field.
[0023] The present invention discloses the following technical effects:
[0024] (1) The metal powder and metal fine wires in the conductive composite frame of the present invention have good conductive properties, which can make the conductive composite frame have the conductive properties of metal, thereby solving the problem that the composite frame cannot conduct electricity.
[0025] (2) The method of the present invention can improve the overall conductivity, mechanical strength and corrosion resistance of the frame. The metal powder and metal wires in the frame are evenly distributed in the frame, providing multiple conductive paths, thereby improving the overall conductivity of the frame. The metal wires in the frame can also enhance the mechanical strength and toughness of the frame. The resin and glass fiber in the frame themselves have good corrosion resistance. Combined with the metal powder and fine wire materials, the corrosion resistance of the frame can be further improved.
[0026] (3) The present invention can make the frame conductive by simply adding metal powder and metal fine wire during the frame forming process, without the need for additional conductive processing steps, thereby simplifying the production process and improving production efficiency.
[0027] (4) The conductive composite frame of the present invention has more excellent conductivity and corrosion resistance, can meet the grounding requirements of the photovoltaic system, and has high stability and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a schematic diagram of the structure of the small sample. DETAILED DESCRIPTION
[0030] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0031] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0032] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0033] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0035] The diameter of the metal thin wire used in the present invention is 5 microns, and the aspect ratio is 50:1; the diameter of the glass fiber is 20 microns, and the length is the same as the length of the conductive composite frame; the particle size of the metal powder is 1 to 10 microns.
[0036] Example 1
[0037] A conductive composite frame:
[0038] The conductive composite frame is composed of the following raw materials, measured by mass percentage: 5% of metal powder (copper powder), 5% of metal fine wire (copper wire), 75% of glass fiber and 15% of resin (polyurethane).
[0039] (1) Mixing process: The metal powder and the metal wire are uniformly mixed into the resin, and then the glass fiber is added for high shear mixing (shear speed is 4000 rpm, mixing time is 25 min, and the temperature is maintained at 25° C.) to obtain a mixture.
[0040] (2) Compression molding: The mixed material is added into a mold preheated to 120°C, and then a pressure of 20 MPa is applied and maintained for 15 min. The temperature is then raised to 150°C, and the pressure is increased to 50 MPa at 150°C and maintained for 35 min to obtain a molded frame.
[0041] (3) Curing treatment: The molded frame is subjected to a heating and curing treatment at a temperature of 70° C. for 2 hours. After the curing is completed, the frame is cooled to obtain a conductive composite frame.
[0042] (4) Application and installation:
[0043] ①Ground wire connection:
[0044] Design connection points: Reserve ground connection points in the design of the conductive composite frame, and use conductive materials to ensure that these connection points are well connected to the internal metal network.
[0045] Install the ground wire: Reliably connect the ground wire to the conductive composite frame through these connection points to ensure that the current can be effectively guided to the ground.
[0046] ②Electrical safety:
[0047] Standards compliance: Ensure that the installed PV panels meet international electrical safety standards and can effectively conduct current in the event of an electrical fault or lightning strike.
[0048] System safety: The conductive composite frame guides the current safely to the ground, reducing the risk of electric shock and fire, and improving the overall safety and reliability of the system.
[0049] Effect Example 1
[0050] 1. Conductive performance test
[0051] (1) Resistance measurement:
[0052] Method: Use a resistance measuring instrument to measure the resistance of the sample to ensure that its conductive performance meets the design requirements.
[0053] Standard: According to the international electrical safety standard (IEC61730), measure the resistance value, record the measurement results, and compare them with the standard requirements to ensure compliance with the specifications.
[0054] (2) Corrosion resistance test:
[0055] Method: Carry out corrosion resistance tests on samples, such as salt spray tests, to simulate the corrosion conditions in the marine environment and verify the corrosion resistance of the samples.
[0056] Objective: To observe the test results and ensure that the samples (such as frames) with added metal (metal powder, metal wire) still maintain excellent corrosion resistance and that the metal's electrical conductivity is not affected by corrosion and does not affect its long-term use in the offshore environment.
[0057] 2. Experimental process:
[0058] (1) Sample preparation: Prepare several processed small samples (cut from the prepared conductive composite frame; the size is generally 300mm×20mm×10mm, see the structural diagram Figure 1 );
[0059] (2) Experimental equipment: volume resistivity tester, TC environmental chamber, HF environmental chamber, DH environmental chamber, salt spray tester, three-point bending tester, tensile tester, impact tester, compression tester;
[0060] (3) Volume resistivity test experimental steps:
[0061] Connect the test circuit: Connect the sample to the precision resistance tester, using the four-terminal method to eliminate the influence of contact resistance. The test circuit includes power supply, standard resistor and sample resistor.
[0062] Measuring Voltage and Current: A known constant current is applied through the electrodes and the voltage drop across the sample is measured. The current and voltage drop data are recorded to calculate the volume resistivity.
[0063] (4) Environmental test (three small samples are used for each type of environmental test):
[0064] 1.TC200 (thermal cycle test):
[0065] ① The component temperature in the aging box cycles between -40±2℃ and 85±2℃, and the temperature change rate does not exceed 100℃ / h. At each extreme temperature, it should remain stable for at least 10 minutes, and one cycle should not exceed 6 hours.
[0066] ② After the test is completed, there is at least 1 hour of recovery time to test performance.
[0067] 2.DH1000 (high temperature and high humidity test):
[0068] ① Test for 1000h at temperature 85±2℃ and relative humidity 85±5%.
[0069] ② After the test is completed, there is at least 2 to 4 hours of recovery time to test performance.
[0070] 3. HF10 (humidity-freeze cycle test):
[0071] ① The sample temperature in the aging box cycles between -40±2℃ and 85±2℃, maintaining at 85℃ for at least 20h, at 85℃ for a maximum of 4h, and at -40℃ for at least 0.5h, for 10 cycles.
[0072] ② At all temperatures above room temperature, maintain relative humidity within 85%±5%; there is no relative humidity control requirement for temperatures below room temperature.
[0073] ③The temperature change rate above 0℃ shall not exceed 100℃ / h, and the temperature change rate below 0℃ shall not exceed 200℃ / h.
[0074] ④ After the test is completed, there is at least 2 to 4 hours of recovery time to test performance.
[0075] 4. Salt spray corrosion test:
[0076] ①Salt spray: salt spray concentration 5±1%, test temperature 15~35℃, spray volume 1~2mL / h / 80cm 2 , pH value 6.5~7.2 at 35±2℃; relative humidity>85%RH.
[0077] ② Sample position: The inclination angle of the upper surface of the component to the vertical direction is 15 to 30°.
[0078] ③Test cycle: The national standard is 96h.
[0079] After the environmental test is completed, its mechanical strength and volume resistivity are tested.
[0080] Table 1 Performance comparison before and after environmental testing
[0081]
[0082] Comparative Example 1
[0083] The same as Example 1, except that the conductive composite frame is composed of the following raw materials, by mass percentage: 12.5% metal powder (copper powder), 12.5% metal fine wire (copper wire), 60% glass fiber and 15% resin (polyurethane).
[0084] The performance of the frame prepared in this comparative example was measured using the same method as in Example 1. The results are shown in Table 2.
[0085] Table 2 Performance comparison before and after environmental testing
[0086]
[0087] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A conductive composite frame, characterized in that: The invention comprises the following raw materials in percentage by mass: 5-10% of metal powder, 5-10% of metal fine wire, 65-85% of glass fiber and 15-35% of resin.
2. The conductive composite frame according to claim 1, characterized in that: The metal powder includes copper powder, aluminum powder or nickel powder; The metal thin wires include copper wires.
3. The conductive composite frame according to claim 1, characterized in that: The resin includes polyurethane or epoxy acrylate.
4. The conductive composite frame according to claim 1, characterized in that: The particle size of the metal powder is 1 to 10 microns; the diameter of the metal wire is 5 microns, and the aspect ratio is 50:1; the diameter of the glass fiber is 20 microns, and the length is the same as that of the conductive composite frame.
5. A method for preparing a conductive composite frame according to any one of claims 1 to 4, characterized in that: The following steps are involved: The raw materials are mixed evenly to obtain a mixture, the mixture is molded and then cured to obtain the conductive composite frame.
6. The preparation method according to claim 5, characterized in that: The compression molding specifically includes: adding the mixed material into a mold preheated to 120° C., then applying a pressure of 20 MPa, maintaining for 10 to 20 minutes, then heating to 150° C., and increasing the pressure to 50 MPa at 150° C., maintaining for 30 to 40 minutes.
7. The preparation method according to claim 5, characterized in that: The curing treatment is performed at a temperature of 60 to 80° C. and for a time of 2 to 4 hours.
8. Use of the conductive composite frame according to any one of claims 1 to 4 in the photovoltaic field.