Silica gel magnetic attraction material of flexible cable and preparation method of silica gel magnetic attraction material

By combining modified magnetic powder with raw rubber and platinum vulcanizer, silicone magnetic absorbing materials with softness, toughness and magnetic absorption are prepared, which solves the problems of breakage and inconvenient storage of data lines during use, and achieves better Experience and durability.

CN118978809AInactive Publication Date: 2024-11-19HUIZHOU YUANSU POLYMER MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411022242.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Although existing silicone materials are soft and tough when applied to data lines, they are prone to breaking and cracking under magnetic absorption due to the increase of magnetic powder, and are inconvenient to storage and length adjustment, which affects the user experience.

Method used

By using 1,3-bis(3-methacryloyloxypropyl)tetra(trimethylsiloxy)disiloxane and/or 3-[tris(1-methylethoxy)silyl] Propyl methacrylate modifies the magnetic powder to form the modified magnetic powder, and combines it with raw glue and platinum vulcanizing agent to prepare a silicone magnetic material with better flexibility, toughness and magnetic absorption.

Benefits of technology

It realizes that the data line is not easy to break or crack during use, and is easy to coil and store through magnetic absorption, reducing distraction, improving the flexibility and toughness of the cable, and enhancing the magnetic absorption effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a silica gel magnetic attraction material of a flexible cable and a preparation method of the silica gel magnetic attraction material. The rubber is prepared from the following raw materials in parts by weight: 70-80 parts of raw rubber, 1-3 parts of a platinum vulcanizing agent, 20-30 parts of modified magnetic powder and 1-5 parts of a filler, the modified magnetic powder is prepared from the following raw materials: alkene siloxane, an alcohol solution and magnetic powder, and the alkene siloxane is 1, 3-bis (3-methacryloyloxypropyl) tetra (trimethylsiloxy) disiloxane and / or 3-[tri (1-methylethyoxyl) silyl] propyl methacrylate. Magnetic powder is modified through 1, 3-bis (3-methacryloyloxypropyl) tetra (trimethylsiloxy) disiloxane and / or 3-[tri (1-methyl ethyoxyl) silyl] propyl methacrylate to obtain modified magnetic powder, the modified magnetic powder is blended with raw rubber and a filler, and under the action of a platinum vulcanizing agent, the modified magnetic powder is subjected to heat treatment to obtain the high-strength magnetic material. The prepared silica gel magnetic attraction material has better softness, toughness and magnetic attraction effect, and the phenomena of fracture, damage and the like are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of silicone rubber, and more specifically, to a silicone magnetic material for a flexible cable and a preparation method thereof. Background Art

[0002] Silicone materials have good softness, elasticity, high temperature resistance, aging resistance, etc., so they are widely used in electronic products, daily necessities, medical equipment, new energy vehicles and other fields. When silicone materials are used in cables in electronic products, such as data cables, the data cables produced are soft and not easy to break or crack due to the good softness of silicone materials. However, during the use of data cables, the data cables are relatively long and difficult to store, which makes them prone to scattering, crisscrossing, etc., affecting their appearance. To solve this problem, some methods use ropes to coil them and then fix them, but when adjusting the length of the data cables, the ropes need to be loosened and then re-fixed, which is more cumbersome. There are also methods that can store data cables by setting up a data cable storage device, which is conducive to adjusting the length, but inconvenient to carry.

[0003] Therefore, currently, magnetic powder is added to the raw material system of silica gel to form silica gel material with magnetic attraction. Due to the magnetic attraction, the data cable produced by silica gel material can be coiled; however, with the large amount of magnetic powder added, the original softness and toughness of the silica gel material are reduced. Therefore, during use or coiling, it is easy to break, crack or fall apart after coiling. Therefore, further research is needed. Summary of the invention

[0004] In order to obtain better softness, toughness and magnetic attraction, the present application provides a silicone magnetic attraction material for a flexible cable and a preparation method thereof.

[0005] In the first aspect, the present application provides a silicone magnetic material for a flexible cable, which is made from the following raw materials in parts by weight: 20-80 parts of raw rubber 1-3 parts of platinum vulcanizing agent Modified magnetic powder 30-75 parts 1-5 portions of filler; The modified magnetic powder is prepared from the following raw materials: olefin siloxane, alcohol solution and magnetic powder; The siloxane is 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and / or 3-[tris(1-methylethoxy)silyl]propyl methacrylate.

[0006] In the above technical scheme, 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tris(1-methylethoxy)silyl]propyl methacrylate both contain multiple reactive groups and multiple siloxy groups. After being hydrolyzed by an alcohol solution, they are used to modify the magnetic powder to form a coating film on the surface of the magnetic powder to obtain a modified magnetic powder. The modified magnetic powder has good compatibility with the polymer and is used in the silicone magnetic material to not only increase the volume, but also promote the close connection between the magnetic powder and the raw rubber molecules, so that the silicone magnetic powder material obtained has good softness, toughness and magnetic attraction.

[0007] Platinum vulcanizer is a two-component addition type silicone platinum vulcanizer, also known as platinum water, A / B two-component. It is a process in which hydrogen-containing silicone oil reacts with vinyl double bonds to form a silylation reaction in the presence of a catalyst, thereby achieving the purpose of crosslinking and vulcanization. Under the action of platinum vulcanizer, the raw rubber and the coating film on the surface of the modified magnetic powder are tightly connected, so that the obtained silicone magnetic powder material has better softness, toughness and magnetic attraction.

[0008] In summary, the magnetic powder is surface treated with 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and / or 3-[tri(1-methylethoxy)silyl]propyl methacrylate to obtain modified magnetic powder, which is then filled in raw rubber. Under the action of platinum vulcanizer and filler, the prepared silicone magnetic material has better softness, toughness and magnetic attraction. The silicone magnetic material is used to produce data cables, which are easy to magnetically coil and store, reducing the possibility of scattering. At the same time, it is not easy to break or damage during use.

[0009] Preferably, the siloxane is composed of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tri(1-methylethoxy)silyl]propyl methacrylate in a weight ratio of 1:(1-5.4).

[0010] When 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tri(1-methylethoxy)silyl]propyl methacrylate are compounded, a synergistic effect is achieved, and the modified magnetic powder obtained is more easily compatible with raw materials such as raw rubber, so that the obtained silicone magnetic material has better softness, toughness and magnetic attraction, reducing the cracking and loosening of data cables produced by silicone magnetic materials.

[0011] Preferably, the magnetic powder is one or more of neodymium iron boron magnetic powder, water atomized iron silicon soft magnetic powder, and sendust soft magnetic powder.

[0012] NdFeB magnetic powder, water-atomized iron silicon soft magnetic powder, and sendust soft magnetic powder all have magnetic attraction; the NdFeB magnetic powder has high coercivity. Water-atomized iron silicon soft magnetic powder is a FeSi compound with excellent energy storage capacity, magnetic induction, corrosion resistance, temperature stability, and small particle size. Sendust soft magnetic powder, also known as FeSiAl alloy powder, is a soft magnetic powder.

[0013] Preferably, the weight ratio of the NdFeB magnetic powder, the water-atomized FeSi soft magnetic powder, and the Sendust soft magnetic powder is (2-6):(1-3):1.

[0014] When NdFeB magnetic powder, water-atomized FeSi soft magnetic powder and FeSiAl soft magnetic powder are compounded and treated with siloxane, the obtained silicone magnetic material has better softness, toughness and magnetic attraction.

[0015] Preferably, the raw rubber is one or more of dihydroxy-terminated polydimethylsiloxane, fluorosilicone raw rubber, 110 raw rubber, 112 raw rubber, and methylphenylvinyl silicone rubber.

[0016] The above raw rubbers can be used with modified magnetic powder, platinum vulcanizer and filler to produce silicone magnetic materials with better softness, toughness and magnetic attraction.

[0017] Preferably, the filler is one or more of white carbon black, calcium carbonate, shell powder and kaolin.

[0018] White carbon black, calcium carbonate, shell powder and kaolin can all play a role in filling and reinforcing, and combined with modified magnetic powder, the prepared silicone magnetic material has better softness, toughness and magnetic attraction.

[0019] Preferably, the alkenyl siloxane is a modified alkenyl siloxane, and the modified alkenyl siloxane is prepared from the following raw materials in parts by weight: 1-3 parts of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane 3-[Tri(1-methylethoxy)silyl]propyl methacrylate 1-3 parts Caprolactone acrylate 0.8-1.5 parts Hydroxyacrylate 2-5 parts Initiator 0.01-0.05 parts Inhibitor 0.001-0.003 parts Ammonium persulfate 0.01-0.05 parts 1-3 parts of anhydrous ethanol 3-5 parts water.

[0020] Both caprolactone acrylate and hydroxy acrylate have good film-forming flexibility and multiple reactive groups. After the compounding reaction, they are further reacted with 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tri(1-methylethoxy)silyl]propyl methacrylate to introduce siloxy groups. The obtained macromolecular grafted polymer can form a coating film with good flexibility and adhesion on the surface of the magnetic powder. The modified magnetic powder obtained is used in the raw material system of silica gel magnetic powder, and has better compatibility, so that the modified magnetic powder is fully mixed with raw materials such as raw rubber, so that the obtained silica gel magnetic material has better flexibility, toughness and magnetic attraction, so that the data cable produced by the silica gel magnetic material can be spirally stored through the magnetic attraction, and is not prone to cracking and breaking during use.

[0021] Preferably, the hydroxy acrylate is one or more of ethylene glycol dimethacrylate, furfuryl methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate.

[0022] Ethylene glycol dimethacrylate, furfuryl methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate all have adhesion and film-forming softness, and caprolactone acrylate works synergistically, and then reacts with 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tri(1-methylethoxy)silyl]propyl methacrylate to form a modified siloxane of a macromolecular grafted polymer, which is used to modify the magnetic powder, so that the prepared modified magnetic powder can be fully mixed with the raw rubber and has good compatibility, thereby further improving the flexibility, toughness and magnetic attraction of the silicone magnetic material.

[0023] The hydroxy acrylate is prepared by compounding ethylene glycol dimethacrylate, furfuryl methacrylate and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate.

[0024] When ethylene glycol dimethacrylate, furfuryl methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate are used to play a synergistic role, the modified magnetic powder obtained has good compatibility with the raw rubber, and the obtained rubber magnetic attraction material has better flexibility, toughness and magnetic attraction.

[0025] Preferably, the modified silane is prepared by the following method: Weigh caprolactone acrylate, hydroxy acrylate, initiator and inhibitor according to weight, mix them evenly, heat to 62-68° C., stir to react, and then add anhydrous ethanol to obtain a graft polymerization solution A; Weigh 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, 3-[tri(1-methylethoxy)silyl]propyl methacrylate, water, and ammonium persulfate in parts by weight, mix well, and hydrolyze for 10-30 minutes to obtain a mixture B; Add 2-3 batches of mixture B to the graft polymerization solution A. After each addition, stir the reaction for 20-30 minutes, cool to 25-35° C., and let stand for 1-2 hours to obtain modified silane.

[0026] In the above scheme, caprolactone acrylate and hydroxy acrylate are subjected to grafting reaction under the action of an initiator, and an inhibitor can reduce the self-polymerization reaction. After heating reaction, a grafted polymer with good flexibility is obtained, which is diluted by anhydrous ethanol to obtain a grafted polymerization solution A.

[0027] 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tri(1-methylethoxy)silyl]propyl methacrylate are hydrolyzed under the action of water, and further grafted with the polymer in the graft polymerization solution A under the action of ammonium persulfate to obtain a macromolecular polymer, which makes it easy to form a coating film on the surface of the magnetic powder, and has good compatibility with the raw material system of the silica gel magnetic material, and can further react with the raw rubber, so that the prepared modified magnetic powder and the raw material of the silica gel magnetic material are evenly dispersed to form a tightly connected molecular structure of the silica gel magnetic powder material, so that the prepared silica gel magnetic powder material has better softness, toughness and magnetic attraction, so that the data cable produced by the silica gel magnetic material can be spirally stored through the magnetic attraction, and is not prone to cracking, breaking and the like during use.

[0028] In a second aspect, the present application provides a method for preparing a silicone magnetic material for a flexible cable, using the following technical solution: Prepared by the following method: 1) Weighing siloxane and alcohol solution and mixing them evenly to obtain a modifier; 2) weighing the modifier and magnetic powder, mixing them, grinding them, and drying them to obtain modified magnetic powder; 3) weighing raw rubber, modified magnetic powder and filler, performing banburying and cooling to obtain a mixed product; 4) The mixed product is mixed with a platinum vulcanizing agent, and kneaded until the platinum vulcanizing agent and the mixed product are fully mixed and uniform, thereby obtaining a silica gel magnetic material.

[0029] In the above process, siloxane and alcohol solution are mixed to hydrolyze siloxane to obtain a modifier, and then the magnetic powder and the modifier are ground to make them fully and evenly mixed, and a modified coating is formed on the surface of the magnetic powder by drying; the modified magnetic powder has good compatibility with the raw rubber raw material, and then combined with platinum vulcanizer and filler, after mixing, kneading, and vulcanization molding, the obtained silicone magnetic material has both good flexibility and magnetic attraction. Therefore, the data cable made of silicone magnetic material can be coiled by magnetic attraction to reduce the phenomenon of scattering, and at the same time has good flexibility and toughness, reducing the possibility of breakage and cracking during use.

[0030] Preferably, a production process for a cable comprises the following steps: According to parts by weight, the silicone magnetic material prepared in the present application is extruded and vulcanized to form a silicone magnetic layer to cover the wire core to obtain a cable.

[0031] In the above process, the operation is simple, and compared with conventional cable production, it saves the need to form a sheath layer on the silicone magnetic layer. The silicone magnetic layer of the present application has better flexibility and magnetic attraction. The obtained cable can be coiled by magnetic attraction, and the possibility of breakage and cracking during use is reduced.

[0032] In addition, the production process of the cable can also be obtained by the following method: According to parts by weight, raw rubber and platinum vulcanizer are weighed and mixed evenly to obtain a sheath material; the sheath material and the silicone magnetic material prepared in the present application are co-extruded and vulcanized to form, so that the formed sheath layer covers the silicone magnetic layer, and the silicone magnetic layer covers the wire core to obtain a cable.

[0033] The cables produced by the above two processes have better softness, toughness and magnetic attraction. Therefore, when the cables are twisted, they can be coiled, which reduces the possibility of cracking and improves the durability of the cables.

[0034] In summary, this application has the following beneficial effects: 1. The surface of magnetic powder is treated with 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and / or 3-[tri(1-methylethoxy)silyl]propyl methacrylate to obtain modified magnetic powder, which is then filled in raw rubber. Under the action of platinum vulcanizer and filler, the prepared silicone magnetic material has better softness, toughness and magnetic attraction. The silicone magnetic material is used to produce data cables, which can be coiled to reduce scattering and are not prone to breakage or damage during use.

[0035] 2. Caprolactone acrylate and hydroxy acrylate both have good film-forming flexibility and have multiple reactive groups. After the compounding reaction, they are further reacted with 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tri(1-methylethoxy)silyl]propyl methacrylate to introduce siloxy groups. The resulting macromolecular grafted polymer can form a coating film with good flexibility and adhesion on the surface of the magnetic powder. The resulting modified magnetic powder is used in the raw material system of silica gel magnetic powder, which has better compatibility, so that the modified magnetic powder is fully mixed with raw materials such as raw rubber, so that the obtained silica gel magnetic absorption material has better flexibility. DETAILED DESCRIPTION

[0036] The present application is further described in detail below with reference to the embodiments.

[0037] Sources of some raw materials: Table 1 Sources of some raw materials Example

[0038] Example 1 A magnetic silica gel material is prepared by the following method: 1) Weigh 2 kg of siloxane and 5 kg of alcohol solution into a stirring device, stir and hydrolyze at a speed of 150 r / min for 30 min to obtain a modifier; 2) Weigh 6 kg of modifier and 25 kg of magnetic powder into a ball mill, grind for 60 min, transfer to an oven at 120° C. and dry for 2 h to obtain modified magnetic powder; 3) Weigh 25 kg of raw rubber, 75 kg of modified magnetic powder and 1 kg of filler into an internal mixer, mix at 150 ° C for 2 h, and cool to 50 ° C to obtain a mixture; 4) The mixed material is transferred to a double-roll mill, and 1 kg of platinum vulcanizing agent is added during the mixing process. The mixing process is continued until the platinum vulcanizing agent and the mixed material are fully mixed to obtain a silica gel magnetic material.

[0039] The raw rubber is dihydroxy-terminated polydimethylsiloxane; the filler is white carbon black; the magnetic powder is neodymium iron boron magnetic powder; the siloxane is 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane; the platinum vulcanizing agent is platinum water; and the alcohol solution is an alcohol solution with a mass fraction of 73%.

[0040] Example 2 The difference between Example 2 and Example 1 is that the amounts of raw materials used in steps 3)-4) are different, as follows: In step 3), 50 kg of raw rubber, 45 kg of modified magnetic powder, and 3 kg of filler; In step 4), 3 kg of platinum vulcanizing agent.

[0041] Example 3 The difference between Example 3 and Example 1 is that the amounts of raw materials used in steps 3)-4) are different, as follows: In step 3), 30 kg of raw rubber, 30 kg of modified magnetic powder, and 5 kg of filler; In step 4), 2 kg of platinum vulcanizing agent.

[0042] Example 4 The difference between Example 4 and Example 2 is that the siloxane is composed of 1 kg 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 1 kg 3-[tris(1-methylethoxy)silyl]propyl methacrylate.

[0043] Example 5 The difference between Example 5 and Example 2 is that the siloxane is composed of 0.6 kg 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 1.4 kg 3-[tris(1-methylethoxy)silyl]propyl methacrylate.

[0044] Example 6 The difference between Example 6 and Example 2 is that the siloxane is composed of 0.3 kg of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 1.7 kg of 3-[tris(1-methylethoxy)silyl]propyl methacrylate.

[0045] Example 7 The difference between Example 7 and Example 5 is that the magnetic powder is composed of 15 kg of neodymium iron boron magnetic powder and 5 kg of water-atomized iron silicon soft magnetic powder.

[0046] Example 8 The difference between Example 8 and Example 5 is that the magnetic powder consists of 10 kg of neodymium iron boron magnetic powder, 5 kg of water-atomized iron silicon soft magnetic powder, and 5 kg of sendustine soft magnetic powder.

[0047] Example 9 The difference between Example 9 and Example 5 is that the magnetic powder consists of 9 kg of neodymium iron boron magnetic powder, 9 kg of water-atomized iron silicon soft magnetic powder, and 2 kg of sendustine soft magnetic powder.

[0048] Example 10 The difference between Example 10 and Example 5 is that the magnetic powder consists of 12 kg of neodymium iron boron magnetic powder, 6 kg of water-atomized iron silicon soft magnetic powder, and 2 kg of sendustine soft magnetic powder.

[0049] Embodiment 11 The difference between Example 11 and Example 9 is that the modified magnetic powder is prepared by the following method: 1.5 kg of caprolactone acrylate, 5 kg of hydroxy acrylate, 0.005 kg of initiator and 0.001 kg of inhibitor were weighed and put into a reactor for uniform mixing, heated to 70° C., stirred at a speed of 120 r / min, and reacted for 2.8 h, and then 5 kg of anhydrous ethanol was added for dilution to obtain a graft polymerization solution A.

[0050] 1 kg of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, 3 kg of 3-[tri(1-methylethoxy)silyl]propyl methacrylate, 3 kg of water, and 0.03 kg of ammonium persulfate were weighed and mixed, and stirred at a speed of 100 r / min to hydrolyze for 10 min to obtain a mixture B.

[0051] The mixture B was added to the graft polymerization solution A in two batches, with an equal amount added each time. After each addition, stirring was continued and the reaction was carried out for 60 minutes. The temperature was then lowered to 30° C., stirring was stopped, and the mixture was allowed to stand for 2 hours to obtain modified vinyl silane.

[0052] The hydroxy acrylate is ethylene glycol dimethacrylate.

[0053] Example 12 The difference between Example 12 and Example 11 is that the amount of raw materials used is different. 1.2 kg caprolactone acrylate, 3.8 kg hydroxy acrylate, 0.004 kg initiator, 0.002 kg inhibitor, 2 kg 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, 1.7 kg 3-[tris(1-methylethoxy)silyl]propyl methacrylate, 4 kg water, 0.02 kg ammonium persulfate.

[0054] Example 13 The difference between Example 13 and Example 11 is that the amount of raw materials used is different. 0.8 kg caprolactone acrylate, 3 kg hydroxy acrylate, 0.003 kg initiator, 0.001 kg inhibitor, 3 kg 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, 1 kg 3-[tris(1-methylethoxy)silyl]propyl methacrylate, 5 kg water, 0.01 kg ammonium persulfate.

[0055] Embodiment 14 The difference between Example 14 and Example 12 is that the hydroxy acrylate is furfuryl methacrylate.

[0056] Embodiment 15 The difference between Example 15 and Example 12 is that the hydroxy acrylate is 2-carbonyl-tetrahydrofuran-3-hydroxy-methylacrylate.

[0057] Example 16 The difference between Example 16 and Example 12 is that the hydroxy acrylate is composed of 2 kg of ethylene glycol dimethacrylate and 1.8 kg of furfuryl methacrylate.

[0058] Embodiment 17 The difference between Example 17 and Example 12 is that the hydroxy acrylate is composed of 2 kg of ethylene glycol dimethacrylate, 0.5 kg of furfuryl acrylate, and 1.3 kg of 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate.

[0059] Embodiment 18 The difference between Example 18 and Example 11 is that caprolactone acrylate is replaced by hydroxy acrylate in an equal amount.

[0060] Embodiment 19 The difference between Example 19 and Example 11 is that an equal amount of hydroxy acrylate is replaced by caprolactone acrylate.

[0061] Embodiment 20 The difference between Example 20 and Example 11 is that 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane is replaced by 3-[tris(1-methylethoxy)silyl]propyl methacrylate in an equal amount.

[0062] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane is replaced by γ-aminopropyltriethoxysilane in an equal amount.

[0063] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane is replaced by an equal amount of aluminate coupling agent DL411.

[0064] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsilyloxy)disiloxane is used in an equal amount to replace tetraisopropyl di(dioctylphosphite)titanate.

[0065] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the modified magnetic powder is neodymium iron boron magnetic powder.

[0066] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that the modified magnetic powder is replaced by raw rubber in equal amounts.

[0067] Application Examples Application Example 1 Application Example 1 A cable production process comprises the following steps: The silicone magnetic material obtained in Example 1 is put into an extruder for extrusion. The extruded silicone magnetic material is used to coat the copper wire, and then vulcanization is performed. The vulcanization is performed at 155°C for 5 minutes, so that the formed silicone magnetic layer coats the wire core. The thickness of the silicone magnetic layer is 0.6mm, and a cable with a diameter of 2.5mm is obtained.

[0068] Application Example 2-25 The difference between Application Example 2-25 and Application Example 1 is that the sources of the silicone magnetic material are different, as shown in Table 2: Table 2 Sources of silicone magnetic materials for application examples 1-25 Application Example 26 The difference between Application Example 26 and Application Example 1 is that the production process of the cable includes the following steps: Weigh 7kg of raw rubber (dihydroxy-terminated polydimethylsiloxane) and 0.1kg of platinum vulcanizer, put them into a double-roll open mill and mix them evenly to obtain a sheath material; put the sheath material and the silicone magnetic material obtained in Example 1 into a twin-screw extruder to extrude them together, the extruded silicone magnetic material covers the copper wire, and the extruded sheath material covers the extruded silicone magnetic material, and then vulcanization molding is carried out, and vulcanization is carried out at 155°C for 5min, so that the formed sheath layer covers the silicone magnetic layer, and the silicone magnetic layer covers the wire core, the thickness ratio of the sheath layer to the silicone magnetic layer is 1:5, the thickness of the silicone magnetic layer is 0.5mm, and a cable with a diameter of 2.5mm is obtained.

[0069] Performance testing The silicone magnetic materials obtained in Examples 1-20 and Comparative Examples 1-5 were placed in a mold, and the mold was then placed in a flat vulcanizer to vulcanize it at 155°C for 5 minutes. After cooling and shaping at room temperature, test samples were obtained and the following performance tests were performed.

[0070] Detection method / test method 1. Elongation The test sample thickness is 1.5 mm, and the breaking strength and elongation are tested according to the test method ASTM D412.

[0071] 2. Hardness The test was conducted with reference to the national standard GB / T 531.1-2008 and with a Shore A hardness tester.

[0072] 3. Magnetic field strength The silica gel magnetic materials obtained in Examples 1-20 and Comparative Examples 1-4 were tested using a high-precision magnetic field tester (Aicos GS-25, Class 1 accuracy).

[0073] The above experiments were tested 5 times and the average value was taken. The specific data are shown in Table 3; Table 3 Experimental data of Examples 1-20 and Comparative Examples 1-5 Combining Example 1 and Comparative Examples 1-3 and Table 3, it can be seen that the elongation and magnetic field strength of Comparative Examples 1-3 are smaller than those of Example 1, and the hardness is greater than that of Example 1, indicating that the modified magnetic powder prepared by the siloxane of the present application is applied to the silicone magnetic material, so that it has better softness, toughness and magnetic attraction effect.

[0074] Combining Example 9 and Examples 11-17 and Table 3, it can be seen that the elongation and magnetic field strength of Examples 11-17 are greater than those of Example 9, and the hardness is smaller than that of Example 1, indicating that the modified silanol prepared by the present application is used to modify the magnetic powder, so that it has better compatibility and good compatibility with raw rubber and filler. Under the action of the catalyst, the obtained silica gel magnetic powder material has better softness, toughness and magnetic attraction.

[0075] 1. Hovering stability The cable obtained in Application Example 1-26 was coiled along the outer edge to make it magnetically attracted and compass-shaped, with an inner diameter of 4 mm and 10 coils to obtain a coiled test sample; Place the coiled test sample horizontally and drop it from a 2-meter high platform. The laboratory temperature is 25℃ and the humidity is 65%. After the drop, check whether the coiled test sample is scattered. If it is scattered, it is recorded as unqualified. If not, it is recorded as qualified.

[0076] 2. Bending resistance After the cable obtained in application example 1-26 is folded in half, it is pressed with a force of 10N, and then released after 5 minutes. Then the side opposite to the folding point of the previous one is folded in half, and then pressed with a force of 10N, and then released after 5 minutes. And so on, after a crease position is folded repeatedly for 100 times, it is placed for 2 minutes, and the surface conditions are recorded. The above specific experimental results are shown in Table 4; Table 4 Experimental results of application examples 1-26 It can be seen from Table 4 that the hovering stability of application examples 1-20 is qualified, while application examples 21-24 are unqualified, which shows that the silicone magnetic material obtained by using embodiments 1-20 of the present application has better magnetic effect and better flexibility, so it is easy to hover and reduce the phenomenon of scattering.

[0077] After being folded in half for many times, the surface of the cable of Application Examples 1-20 is smooth, and after being folded in half for many times, the surface of the cable of Application Examples 21-24 has creases / cracks, which indicates that the silicone magnetic material obtained in Examples 1-20 can be used in cables to reduce the occurrence of creases, cracks and the like, and improve the durability of the cables.

[0078] In addition, it can be seen from Table 4 that the hovering stability of Application Example 1 and Application Example 26 are both qualified, and their surfaces are smooth after being folded many times, indicating that the effect of using the silicone magnetic material prepared in this application to coat the copper core with a single layer is similar to that of using a double layer to coat the copper core. Based on production efficiency and production cost, the cable production scheme of Application Example 1 is preferably selected in actual production.

[0079] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A silicone magnetic material for a flexible cable, characterized in that: It is prepared from the following raw materials in parts by weight: 25-50 parts of raw rubber 1-3 parts of platinum vulcanizing agent Modified magnetic powder 30-75 parts 1-5 portions of filler; The modified magnetic powder is prepared from the following raw materials: olefinic siloxane, alcohol solution and magnetic powder; the olefinic siloxane is 1,3-bis(3-methacryloxypropyl)tetra(trimethylsiloxy)disiloxane and / or 3-[tri(1-methylethoxy)silyl]propyl methacrylate.

2. The silicone magnetic material for a flexible cable according to claim 1, characterized in that: The siloxane is composed of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane and 3-[tri(1-methylethoxy)silyl]propyl methacrylate in a weight ratio of 1:(1-5.4).

3. The silicone magnetic material for a flexible cable according to claim 1, characterized in that: The magnetic powder is one or more of neodymium iron boron magnetic powder, water atomized iron silicon soft magnetic powder, and sendust soft magnetic powder.

4. The silicone magnetic material for a flexible cable according to claim 3, characterized in that: The weight ratio of the NdFeB magnetic powder, the water-atomized FeSi soft magnetic powder and the Sendust soft magnetic powder is (2-6): (1-3):

1.

5. The silicone magnetic material for a flexible cable according to claim 1, characterized in that: The raw rubber is one or more of dihydroxy-terminated polydimethylsiloxane, fluorosilicone raw rubber, 110 raw rubber, 112 raw rubber, and methylphenyl vinyl silicone rubber.

6. The silicone magnetic material for a flexible cable according to claim 1, characterized in that: The filler is one or more of white carbon black, calcium carbonate, shell powder and kaolin.

7. The silicone magnetic material for a flexible cable according to claim 1, characterized in that: The alkenyl siloxane is a modified alkenyl siloxane, and the modified alkenyl siloxane is prepared from the following raw materials in parts by weight: 1-3 parts of 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane 3-[Tri(1-methylethoxy)silyl]propyl methacrylate 1-3 parts Caprolactone acrylate 0.8-1.5 parts Hydroxyacrylate 2-5 parts Initiator 0.01-0.05 parts Inhibitor 0.001-0.003 parts Ammonium persulfate 0.01-0.05 parts 1-3 parts of anhydrous ethanol 3-5 parts water.

8. The silicone magnetic material for a flexible cable according to claim 7, characterized in that: The hydroxy acrylate is one or more of ethylene glycol dimethacrylate, furfuryl methacrylate, and 2-carbonyl-tetrahydrofuran-3-hydroxy-methacrylate.

9. The silicone magnetic material for a flexible cable according to claim 7, characterized in that: The modified silane is prepared by the following method: Weigh caprolactone acrylate, hydroxy acrylate, initiator and inhibitor according to weight, mix them evenly, heat to 60-68° C., stir to react, and then add anhydrous ethanol to obtain a graft polymerization solution A; Weigh 1,3-bis(3-methacryloxypropyl)tetrakis(trimethylsiloxy)disiloxane, 3-[tri(1-methylethoxy)silyl]propyl methacrylate, water, and ammonium persulfate in parts by weight, mix well, and hydrolyze for 10-30 minutes to obtain a mixture B; Add 2-3 batches of mixture B to the graft polymerization solution A. After each addition, stir the reaction for 20-30 minutes, cool to 25-35° C., and let stand for 1-2 hours to obtain modified silane.

10. A method for preparing the silicone magnetic material for a flexible cable according to any one of claims 1 to 8, characterized in that: Prepared by the following method: 1) Weigh siloxane and alcohol solution and mix them evenly to obtain a modifier; 2) Weigh the modifier and magnetic powder, mix them, grind them, and dry them to obtain modified magnetic powder; 3) Weigh the raw rubber, modified magnetic powder and filler, perform internal kneading, and cool to obtain a mixed product; 4) The mixed material is mixed with a platinum vulcanizer and kneaded until the platinum vulcanizer and the mixed material are fully and evenly mixed to obtain a silicone magnetic material.

Citation Information

Patent Citations

  • Preparing method of modified neodymium-iron-boron magnetic powder, modified neodymium-iron-boron magnetic powder and neodymium-iron-boron sintering body

    CN108231310A

  • Heat-conducting and wave-absorbing material and preparation method thereof

    CN108276773A

  • Curable silicone composition for the production of composite soft magnetic materials, and composite soft magnetic materials

    KR1020050016398A