Structure-reconstructed pyrolytic carbon black and preparation method and device thereof

By consolidating the applied carbon source to the surface of pyrolytic carbon black under high temperature conditions, new pore structures and chemical functional groups are formed, the problem of low structural degree of pyrolytic carbon black is solved, and its binding performance with rubber composite materials is significantly improved , meets the tire usage requirements and realizes resource recycling.

CN118978816AActive Publication Date: 2024-11-19QINGDAO UNIV OF SCI & TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411069580.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The prior art cannot effectively improve the structural degree of pyrolytic carbon black, resulting in insufficient bonding performance in rubber composite materials and cannot meet the tire usage requirements.

Method used

The added carbon source is consolidated to the surface of the pyrolytic carbon black under high temperature conditions to form new pore structures and chemical functional groups. The structure and surface microchemical environment of the pyrolytic carbon black are reshaped through plasma discharge and acid solution immersion and other processes. , improve its bonding performance with rubber composite materials.

Benefits of technology

The binding performance of pyrolytic carbon black and rubber composite materials is significantly improved, with a 300% fixed-extension strength reaching 18.65MPa, which meets the tire usage requirements and realizes resource recycling in the tire life cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978816A_ABST
    Figure CN118978816A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of recycling of solid wastes, and relates to structure-reconstructed pyrolytic carbon black and a preparation method and device thereof.The preparation method comprises the steps that in a protective gas atmosphere, at the temperature of 830-980 DEG C, an external carbon source, pyrolytic carbon black and a reaction initiating active carrier make full contact for 5-12 s, and modified pyrolytic carbon black is obtained; under the condition that the temperature is 450 to 550 DEG C, treating for 1 to 3 minutes through the discharge power of 200 to 400W plasma; then, placing in a 4-9 mol / L acid solution, and soaking for 5-15 minutes; wherein the carbon source is any one of gaseous hydrocarbon, high-carbon-content polymer or thermosetting resin; and the initiation reaction active carrier is a copper foil carrier. By adopting the method and the device, the external carbon source is consolidated to the surface of the pyrolytic carbon black under a high-temperature condition to form a new pore structure and chemical functional groups, the structure and surface micro-chemical environment of the pyrolytic carbon black are remodeled, and the bonding performance of the pyrolytic carbon black and a rubber composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid waste recycling, and specifically relates to a structurally reconstructed pyrolytic carbon black and a preparation method and device thereof, in particular to the pyrolytic carbon black obtained by pyrolysis of waste tires, the structure and surface microchemical environment of which are reshaped to increase the bonding performance of the pyrolytic carbon black and rubber composite materials. Background Art

[0002] As the number of cars in my country continues to increase, the annual production of waste tires has increased year by year, causing serious waste of energy resources and environmental pollution. Pyrolysis can convert waste tires into aromatic-rich oil, high-fuel-value gas, and reusable carbon black and steel wire, which can achieve maximum energy recovery and resource reuse of waste tires. It is currently the most effective way to process waste tires. Compared with other final treatment methods for waste tires, it has the advantages of large processing capacity, high economic benefits, and low pollution. At present, the United States and some European countries have banned incineration, landfilling, and stacking, and only allow pyrolysis, believing that pyrolysis is the most effective and thorough treatment method.

[0003] Pyrolytic carbon black is the second largest product of waste tire pyrolysis, accounting for about 30-35%. Its composition is very complex, mainly containing fillers (carbon black, white carbon black) added in the tire manufacturing process, vulcanization aids (zinc oxide) and reaction derivatives produced in the cracking process (zinc oxide reacts with sulfur to form zinc sulfide and other substances). It has many impurities and low activity. Compared with industrial carbon black, it has large particle size, low structure, and low surface activity, which makes it impossible to reuse it in the preparation process of new tires. Therefore, it is necessary to modify pyrolytic carbon black before reuse.

[0004] There are many methods for activation and modification of pyrolytic carbon black, and a large number of patents have been reported. However, the methods involved are basically to remove impurities and activate the pyrolytic carbon black obtained. Although the strength of the treated pyrolytic carbon black has been improved to a certain extent when preparing rubber composite materials, its 300% tensile strength is still very low and cannot meet the requirements of tire use. The 300% tensile strength is mainly related to the structural degree of the pyrolytic carbon black itself. The higher the structural degree of the pyrolytic carbon black, the greater the value of its 300% tensile strength. Based on the correlation between material properties and material structure, it can be clearly recognized that the current methods and process means for treating pyrolytic carbon black have failed to fundamentally solve the problem of low structural degree of pyrolytic carbon black. Summary of the invention

[0005] The purpose of the present invention is to solve the above-mentioned problems existing in the prior art, and proposes a structurally reconstructed pyrolytic carbon black and a preparation method and device thereof. The present invention consolidates an external carbon source to the surface of the pyrolytic carbon black under high temperature conditions to form a new pore structure and chemical functional groups, reshape the pyrolytic carbon black structure and surface microchemical environment, and increase the bonding performance of the pyrolytic carbon black and rubber composite materials.

[0006] The technical solution of the present invention is:

[0007] The present invention provides a method for preparing structurally reconstructed pyrolytic carbon black, wherein the preparation method is to fix an external carbon source to the surface of the pyrolytic carbon black under certain temperature conditions to form a new pore structure and chemical functional groups, and to reshape the structure and surface microchemical environment of the pyrolytic carbon black, and comprises the following steps:

[0008] S1: In a protective gas atmosphere, the temperature is set to 830-980°C, and the added carbon source, pyrolytic carbon black and the initiating reaction active carrier are fully contacted for 5-12 seconds, a new pore structure grows on the surface of the pyrolytic carbon black, the morphology of the primary particles of the pyrolytic carbon black is changed, and new chemical functional groups are formed on the surface of the pyrolytic carbon black to obtain modified pyrolytic carbon black;

[0009] The number of surface chemical functional groups of the modified pyrolytic carbon black in step S1 is mainly related to the residence time of the carbon source on the surface of the pyrolytic carbon black. The carbon source and the pyrolysis carbon black will fully contact to form functional groups on the surface of the pyrolysis carbon black (the optimal residence time is 2 to 5 seconds). The carbon source used in the present invention includes gaseous and solid carbon sources, but when the carbon source is in gaseous form, it is only necessary to increase its temperature to certain conditions and allow it to decompose and react with the pyrolysis carbon black. However, when the carbon source is in solid form, it is necessary to first decompose to produce a gaseous carbon source and then react with the pyrolysis carbon black. The graded reaction process takes time, so it will be longer than the residence time of 2 to 5 seconds, so the reaction time is set to 5 to 12 seconds.

[0010] The above reaction temperature is any temperature value within the range of 830-980°C, for example, it can be 830°C, 850°C, 870°C, 880°C, 890°C, 895°C, 900°C, 910°C, 920°C, 925°C, 940°C, 950°C, 970°C, or 980°C, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0011] The contact time is any value within the range of 5 to 12 seconds, for example, 5 seconds, 6 seconds, 7 seconds, 8 seconds, 9 seconds, 10 seconds, 11 seconds or 12 seconds, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0012] S2: treating the modified pyrolytic carbon black at a temperature of 450 to 550° C. with a plasma discharge power of 200 to 400 W for 1 to 3 minutes; step S2 improves the orderly distribution characteristics of the carbon structure through local oxidation and etching, increases its activity, and enriches its surface active functional groups.

[0013] S3: placing the treated modified pyrolytic carbon black in an acid solution with a concentration of 4 to 9 mol / L and soaking for 5 to 15 minutes;

[0014] The concentration of the acidic solution is any value within the range of 4 to 9 mol / L, for example, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L or 9 mol / L, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0015] The soaking time is any time within the range of 5 to 15 minutes, for example, it can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0016] S4: Dry;

[0017] S5: Supercritical carbon dioxide is fully mixed with restructured pyrolytic carbon black and sprayed out with a special nozzle. The strong high-frequency pulsating shear force field formed by the rapid expansion of supercritical carbon dioxide is used to refine the particle size of pyrolytic carbon black, and finally restructured pyrolytic carbon black is obtained;

[0018] Wherein, the carbon source is any one of gaseous hydrocarbons, high carbon content polymers or thermosetting resins;

[0019] The initiation reaction active carrier is a copper foil carrier; it should be particularly noted that under different initiation reaction active carrier conditions, the method of the present invention will produce modified pyrolytic carbon black with completely different properties. The new chemical functional group types formed on the surface of the pyrolytic carbon black of the present invention are formed under the conditions of the initiation reaction active carrier based on copper foil. If the initiation reaction active carrier of other systems is replaced, different chemical functional group types will be formed.

[0020] The present invention adopts the above-mentioned preparation method, which can consolidate the added carbon source to the surface of pyrolytic carbon black, grow a new pore structure on the surface of pyrolytic carbon black, change the morphology of primary particles of pyrolytic carbon black, and form new chemical functional groups on the surface of pyrolytic carbon black.

[0021] Furthermore, the protective gas atmosphere is an inert gas atmosphere, including nitrogen and argon;

[0022] The gaseous hydrocarbons are selected from gaseous hydrocarbons having a carbon content of more than 90%, including methane;

[0023] The high carbon content polymer includes any one of polyethylene, polypropylene, polystyrene or a mixture of several of them.

[0024] Furthermore, when the carbon source is a gaseous hydrocarbon, the gaseous hydrocarbon is continuously introduced at an intake rate of 20 ml / min, and in an argon protective gas atmosphere, the gaseous hydrocarbon, the pyrolytic carbon black and the initiating reaction active carrier are fully contacted for 5 to 10 seconds at a heating rate of 10 to 15 K / min and a final temperature of 900 to 950° C.;

[0025] The heating rate is any rate within the range of 10 to 15 K / min, for example, 10 K / min, 11 K / min, 12 K / min, 13 K / min, 14 K / min or 15 K / min, but is not limited to the listed values, and other values ​​not listed within the range are also applicable. Among them, the optimal heating rate is 13 K / min.

[0026] The reaction temperature is preferably 930°C.

[0027] The contact time is any value within the range of 5 to 10 seconds, for example, 5 seconds, 6 seconds, 7 seconds, 8 seconds, 9 seconds or 10 seconds, but is not limited to the listed values, and other values ​​not listed within the range are also applicable. Among them, the optimal contact time is 8 seconds.

[0028] When the carbon source is a high carbon content polymer, the mass ratio of the high carbon content polymer to the pyrolytic carbon black is 1.5 to 2:100, and the pyrolytic carbon black is fully contacted with the decomposition product of the high carbon content polymer and the initiation reaction active carrier for 8 to 12 seconds at a heating rate of 5 to 10 K / min and a final temperature of 830 to 880° C. in an argon protective gas atmosphere;

[0029] The above mass ratio of 1.5 to 2:100 may be 1.5:100, 1.6:100, 1.7:100, 1.8:100, 1.9:100 or 1:50, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0030] The heating rate is any rate within the range of 5 to 10 K / min, for example, 5 K / min, 6 K / min, 7 K / min, 8 K / min, 9 K / min or 10 K / min, but is not limited to the listed values, and other values ​​not listed within the range are also applicable. Among them, the optimal heating rate is 8 K / min.

[0031] The reaction temperature is preferably 850°C.

[0032] The contact time is any value within the range of 8 to 12 seconds, for example, 8 seconds, 9 seconds, 10 seconds, 11 seconds or 12 seconds, but is not limited to the listed values, and other values ​​not listed within the range are also applicable. Among them, the optimal contact time is 10 seconds.

[0033] When the carbon source is a thermosetting resin, the mass ratio of the thermosetting resin to the pyrolytic carbon black is 2.5-3.5:100. In a nitrogen protective gas atmosphere, at a heating rate of 2-5 K / min and a final temperature of 950-980° C., the pyrolytic carbon black is fully contacted with the decomposition product of the thermosetting resin and the initiation reaction active carrier for 5-8 seconds.

[0034] The above mass ratio of 2.5 to 3.5:100 can be 2.5:100, 2.6:100, 2.7:100, 2.8:100, 2.9:100, 3.0:100, 3.1:100, 3.2:100, 3.3:100, 3.4:100 or 3.5:100, but is not limited to the listed values, and other unlisted values ​​within the range are equally applicable.

[0035] The heating rate is any rate within the range of 2 to 5 K / min, for example, 2 K / min, 3 K / min, 4 K / min or 5 K / min, but is not limited to the listed values, and other values ​​not listed within the range are also applicable. Among them, the optimal heating rate is 3 K / min.

[0036] The reaction temperature is preferably 970°C.

[0037] The contact time is any value within the range of 5 to 8 seconds, for example, 5 seconds, 6 seconds, 7 seconds or 8 seconds, but is not limited to the listed values, and other values ​​not listed within the range are also applicable. Among them, the optimal contact time is 7 seconds.

[0038] Furthermore, in the step S1, the added carbon source is solidified to the surface of the pyrolytic carbon black to form chemical functional groups; the formation of new chemical functional groups on the surface of the pyrolytic carbon black is closely related to the carbon source form and the structural reconstruction process; when gaseous hydrocarbons are used as the carbon source, under the above reaction conditions, the functional groups are mainly hydroxyl groups; when high carbon content polymers are used as the carbon source, under the above reaction conditions, the functional groups are mainly hydroxyl groups and amide groups; when thermosetting resins are used as the carbon source, under the above reaction conditions, the functional groups are mainly hydroxyl groups and aromatic groups.

[0039] Furthermore, the step S2 partially oxidizes the modified pyrolytic carbon black, that is, the surface carbon source structure of the modified pyrolytic carbon black is strengthened by plasma at a certain temperature; comprising:

[0040] The modified pyrolytic carbon black is treated at 450°C for 3 min by a plasma discharge power of 200 W; or,

[0041] The modified pyrolytic carbon black is treated at 500°C for 2 min by a plasma discharge power of 300 W; or,

[0042] The modified pyrolytic carbon black was treated at 550°C for 1 min by a plasma discharge power of 400 W.

[0043] Furthermore, in step S3, the modified pyrolytic carbon black is etched, and the acidic solution is one or both of sulfuric acid and hydrofluoric acid;

[0044] Wherein, under the condition of sulfuric acid: its concentration is 5-9 mol / L, and the soaking time is 10-15 min; preferably, the optimal concentration is 7 mol / L, and the optimal soaking time is 12 min.

[0045] Under the condition of hydrofluoric acid: the concentration is 4-7 mol / L, and the immersion time is 5-10 min; preferably, the optimal concentration is 5 mol / L, and the optimal immersion time is 7 min.

[0046] After new chemical functional groups are formed on the surface of pyrolytic carbon black, the above-mentioned local oxidation and etching can improve the orderly distribution characteristics of the carbon structure, increase its activity, and enrich its surface active functional groups.

[0047] The present invention also provides a restructured pyrolytic carbon black prepared by any of the preparation methods described above.

[0048] The preparation method of structurally reconstructed pyrolytic carbon black provided by the present invention controls multiple process parameters such as adjustment and optimization of the addition ratio of pyrolytic carbon black and external carbon source, regulation of reaction atmosphere, optimization of reaction temperature, adjustment of reaction time, optimization of partial oxidation and etching conditions, etc. under the action of external multi-field strengthening, so that the size of the pore structure, growth thickness, and types and quantities of surface chemical functional groups on the surface of the pyrolytic carbon black can be controlled.

[0049] The external multi-field strengthening mentioned above refers to the introduction of multiple fields such as magnetic field, ultrasound, plasma, etc. during the treatment of pyrolytic carbon black to activate the gas around the surface growth of pyrolytic carbon black, change the structure and reshape the aggregation state evolution of pyrolytic carbon black, thereby achieving the effect of strengthening the structural remodeling of pyrolytic carbon black.

[0050] The multi-process parameter control mentioned above is to adjust the pyrolytic carbon black structural reconstruction process parameters according to the performance requirements of the target product pyrolytic carbon black, such as structural degree, aggregate structure, chemical composition, surface morphology, and properties of surface chemical groups.

[0051] The performance requirements of the target product pyrolytic carbon black structure are mainly achieved by adjusting the addition ratio of pyrolytic carbon black to external carbon source, reaction atmosphere and reaction temperature process parameters.

[0052] The performance requirements of the aggregated structure of the target product pyrolysis carbon black are mainly determined by the process parameters such as reaction time, reaction atmosphere, reaction temperature, and local oxidation and etching conditions.

[0053] The performance requirements of the chemical composition of the target product pyrolytic carbon black are mainly achieved by adjusting the addition ratio of pyrolytic carbon black to external carbon source, reaction atmosphere, reaction temperature and process parameters.

[0054] The performance requirements of the surface morphology of the target product pyrolysis carbon black are mainly achieved by adjusting the process parameters such as reaction time, reaction temperature, local oxidation and etching conditions.

[0055] The performance requirements of the surface chemical group properties of the target product pyrolytic carbon black are mainly achieved by adjusting the process parameters of local oxidation and etching conditions.

[0056] Furthermore, the restructured pyrolytic carbon black is mixed with rubber to prepare a restructured pyrolytic carbon black rubber composite material.

[0057] In order to increase the bonding performance of pyrolytic carbon black and rubber composite materials, the present invention also needs to cooperate with the mixing process for preparing the restructured pyrolytic carbon black rubber composite material; during the mixing process of the composite material, small materials, rubber, and white carbon black need to be added according to the composite material formula, and then the restructured pyrolytic carbon black and operating oil are added to the mixing system. After the mixing temperature reaches 155°C, the glue is discharged and the material is cooled.

[0058] The present invention also provides a device for implementing any of the preparation methods described above, characterized in that the device comprises a continuous feeding extruder, a device body and a continuous discharging extruder connected in sequence, and a transmission assembly and a bearing assembly are fixedly installed on the device body; the device body comprises a shell, an electric heating coil is installed on the shell, a conveying assembly and a protective gas channel are arranged inside the shell, the conveying assembly is made of copper foil material, and the protective gas channel is installed in the middle and upper position of the conveying assembly; the continuous feeding extruder is inserted into the device body and extends to just above the conveying assembly; a conveying assembly main drive wheel and a conveying assembly driven drive wheel are respectively arranged at both ends of the conveying assembly, and the transmission assembly drives the bearing assembly and the conveying assembly main drive wheel to rotate, thereby driving the conveying assembly and the conveying assembly driven drive wheel to rotate at a uniform speed; the device is also provided with a sealing assembly.

[0059] Furthermore, the continuous discharging extruder is fixedly connected to the device body and forms an angle of 45 degrees with the shell;

[0060] The shell is also provided with a protective gas inlet and a protective gas outlet, and the protective gas inlet and the protective gas outlet are respectively connected to the two ends of the protective gas channel;

[0061] The protective gas channel is installed at a position 20% above the middle of the conveying component;

[0062] A sealing assembly is provided at a position where the shell cooperates with the main transmission wheel of the conveying assembly and the driven transmission wheel of the conveying assembly. The sealing assembly includes a shell side wall, a transmission wheel center axis and a sealing dynamic ring that is interference fit with the transmission wheel center axis. The sealing dynamic ring is a U-shaped structure, and the sealing working plane of the sealing dynamic ring exceeds the working surface of the transmission wheel center axis by 1 to 2 mm. A static sealing upper ring and a static sealing lower ring are provided at a position where the shell side wall and the sealing dynamic ring cooperate. Both the static sealing upper ring and the static sealing lower ring are circular rings. The static sealing upper ring is 10 mm longer than the static sealing lower ring. A sealing ring is provided between the sealing dynamic ring and the static sealing upper ring and the static sealing lower ring. The sealing assembly also includes a lubricating oil port.

[0063] Beneficial effects of the present invention:

[0064] The present invention fixes the added carbon source to the surface of pyrolytic carbon black under high temperature conditions to form a new pore structure and chemical functional groups, reshape the pyrolytic carbon black structure and surface microchemical environment, and increase the bonding performance of pyrolytic carbon black and rubber composite materials. Moreover, according to the performance requirements of the rubber composite material, under the action of external multi-field reinforcement, the pyrolytic carbon black and the added carbon source ratio can be adjusted and optimized, the reaction atmosphere is controlled, the reaction temperature is optimized, the reaction time is adjusted, and the local oxidation and etching conditions are optimized. The pore structure size, growth thickness, and the types and quantities of surface chemical functional groups of the pyrolytic carbon black surface can be controlled, and a complete set of pyrolytic carbon black structure reconstruction equipment has been developed, which is currently being promoted and applied industrially.

[0065] The present invention realizes the transformation of the tire life cycle from the linear model of "resources-products-waste" to the circular model of "resources-products-renewable resources", which is of great significance for promoting the construction of ecological civilization in my country and building a resource-saving and environmentally friendly society. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 A schematic diagram of the structure of the device provided by the present invention;

[0067] Figure 2 A cross-sectional view of the device structure provided by the present invention;

[0068] Figure 3 A schematic diagram of the structure of the sealing assembly provided by the present invention;

[0069] In the above figures, Ⅰ, continuous feeding extruder; Ⅱ, device body; Ⅲ, continuous discharging extruder; Ⅳ, frame; 1, sealing assembly; 2, protective gas inlet; 3, protective gas outlet; 4, bearing assembly; 4-1, sealing dynamic ring; 4-2, sealing ring; 4-3, static sealing upper ring; 4-4, static sealing lower ring; 5, transmission assembly; 6, housing; 6-1, housing side wall; 6-2, lubricating oil port; 7, protective gas channel; 8, conveying assembly; 9, conveying assembly main drive wheel; 9-1, drive wheel center axis; 10, conveying assembly driven drive wheel. DETAILED DESCRIPTION

[0070] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0071] Example 1

[0072] In this embodiment, gaseous hydrocarbons are used as the carbon source, and the structure of pyrolytic carbon black is reconstructed under this condition.

[0073] (1) Pyrolysis carbon black structure reconstruction process:

[0074] S1: In the process of pyrolytic carbon black structural reconstruction, methane is used as the carbon source. The methane is continuously introduced into the reaction device at a gas intake rate of 20 ml / min. In an argon protective gas atmosphere, the heating rate is 13 K / min, and the final temperature is 950 ° C. The methane and pyrolytic carbon black are fully contacted on the copper foil carrier for 10 seconds.

[0075] S2: treating the modified pyrolytic carbon black produced in step S1 at a temperature of 450° C. with a plasma discharge power of 200 W for 3 min;

[0076] S3: Soak the modified pyrolytic carbon black treated in step S2 in 7 mol / L sulfuric acid for 12 minutes.

[0077] S4: Drying the modified pyrolytic carbon black prepared in step S3.

[0078] (2) Preparation process of structurally reconstructed pyrolytic carbon black rubber composite materials:

[0079] S1: The modified pyrolytic carbon black prepared by the pyrolytic carbon black structural reconstruction is weighed according to the requirements of the rubber composite material formula; the formula components and the number of parts are shown in Table 1 below:

[0080] Table 1 Name and quantity of each component in the formula

[0081]

[0082]

[0083] S2: Mixing process parameters are set as follows:

[0084] The mixing chamber temperature is 60°C, the speed is 60r / min, the filling factor is 0.65, and the upper push bolt pressure is 0.7MPa;

[0085] S3: The mixing process is:

[0086] First add rubber, mix for 40 seconds, then add zinc oxide ZnO, stearic acid SAD, accelerator 4020, antioxidant RD, microcrystalline wax, plasticizer A; after mixing for 40 seconds, add coupling agent Si69 and precipitated silica; after mixing for 40 seconds, slowly and in multiple times add pyrolysis carbon black and operating oil; after mixing for 40 seconds, lift the plug, and finally mix to 155°C for rubber removal.

[0087] S4: The rubber compound mixed in S3 is sheeted and vulcanized, and then the properties of the rubber compound are tested.

[0088] (3) Test results

[0089] Table 1 Performance test data of structurally regenerated pyrolytic carbon black

[0090] project Pyrolytic Carbon Black Restructured Pyrolytic Carbon Black <![CDATA[Iodine absorption value / g·kg -1 > 85 140 <![CDATA[DBP oil absorption value / 10 -5 m 3 .kg -1 > 90 100 <![CDATA[Nitrogen adsorption specific surface area (NSA) / 10 3 m 2 .kg -1 > 26.87 46.3 Add or subtract calories / % 3.02 0.05 Subdivision content / % 40.6 7.26 Particle hardness 51 45.5 325 mesh screen residue / % 0.05 0.05

[0091] Table 2 Performance analysis of rubber composite materials

[0092] Pyrolytic carbon black rubber composites Structural Reconstruction of Pyrolytic Carbon Black Rubber Composites hardness 54.5 58.3 100% fixed stretch 1.82 2.88 200% fixed stretch 5.14 8.26 300% fixed stretch 10.78 13.55 Tensile Strength 22.94 22.38 Elongation at break 476.77 501.08 Tensile product 10933 11214

[0093] Example 2

[0094] In this example, a high carbon content polymer is used as a carbon source, and the pyrolytic carbon black is restructured under this condition.

[0095] (1) Pyrolysis carbon black structure reconstruction process:

[0096] S1: In the process of pyrolytic carbon black structural reconstruction, polyethylene is used as the carbon source. In an argon protective gas atmosphere, at a heating rate of 8K / min, and at a final temperature of 850°C, pyrolytic carbon black with a mass ratio of 1.8:100 and polyethylene decomposition products are fully contacted on a copper foil carrier for 10 seconds.

[0097] S2: treating the modified pyrolytic carbon black produced in step S1 at a temperature of 500° C. with a plasma discharge power of 300 W for 2 min;

[0098] S3: Soak the modified pyrolytic carbon black treated in step S2 in 7 mol / L sulfuric acid for 12 minutes.

[0099] S4: Drying the modified pyrolytic carbon black prepared in step S3.

[0100] (2) Preparation process of structurally reconstructed pyrolytic carbon black rubber composite materials:

[0101] S1: The modified pyrolytic carbon black prepared by structural reconstruction of pyrolytic carbon black is weighed according to the requirements of the rubber composite material formula; the formula components and the number of parts are shown in Table 1 in Example 1.

[0102] S2: Mixing process parameters are set as follows:

[0103] The mixing chamber temperature is 60°C, the speed is 60r / min, the filling factor is 0.65, and the upper push bolt pressure is 0.7MPa;

[0104] S3: The mixing process is:

[0105] First add rubber, mix for 40 seconds, then add zinc oxide ZnO, stearic acid SAD, accelerator 4020, antioxidant RD, microcrystalline wax, plasticizer A; after mixing for 40 seconds, add coupling agent Si69 and precipitated silica; after mixing for 40 seconds, slowly and in multiple times add pyrolysis carbon black and operating oil; after mixing for 40 seconds, lift the plug, and finally mix to 155°C for rubber removal.

[0106] S4: The rubber compound mixed in S3 is sheeted and vulcanized, and then the properties of the rubber compound are tested.

[0107] (3) Test results

[0108] Table 3 Performance test data of structurally regenerated pyrolytic carbon black

[0109] project Pyrolytic Carbon Black Restructured Pyrolytic Carbon Black <![CDATA[Iodine absorption value / g·kg -1 > 85 152 <![CDATA[DBP oil absorption value / 10 -5 m 3 .kg -1 > 90 105 <![CDATA[Nitrogen adsorption specific surface area (NSA) / 10 3 m 2 .kg -1 > 26.87 42.9 Add or subtract calories / % 3.02 0.07 Subdivision content / % 40.6 9.26 Particle hardness 51 47.6 325 mesh screen residue / % 0.05 0.05

[0110] Table 4 Performance analysis of rubber composite materials

[0111]

[0112]

[0113] Example 3

[0114] In this embodiment, thermosetting resin is used as a carbon source, and the structure of pyrolytic carbon black is reconstructed under this condition.

[0115] (1) Pyrolysis carbon black structure reconstruction process:

[0116] S1: In the process of pyrolytic carbon black structural reconstruction, acrylic resin is used as the carbon source. In a nitrogen protective gas atmosphere, at a heating rate of 3K / min and a final temperature of 980°C, pyrolytic carbon black with a mass ratio of 3:100 and the decomposition product of acrylic resin are fully contacted on a copper foil carrier for 8 seconds.

[0117] S2: treating the modified pyrolytic carbon black produced in step S1 at a temperature of 550°C with a plasma discharge power of 400W for 1 min;

[0118] S3: Soak the modified pyrolytic carbon black treated in step S2 in 7 mol / L sulfuric acid for 12 minutes.

[0119] S4: Drying the modified pyrolytic carbon black prepared in step S3.

[0120] (2) Preparation process of structurally reconstructed pyrolytic carbon black rubber composite materials:

[0121] S1: The modified pyrolytic carbon black prepared by structural reconstruction of pyrolytic carbon black is weighed according to the requirements of the rubber composite material formula; the formula components and the number of parts are shown in Table 1 in Example 1.

[0122] S2: Mixing process parameters are set as follows:

[0123] The mixing chamber temperature is 60°C, the speed is 60r / min, the filling factor is 0.65, and the upper push bolt pressure is 0.7MPa;

[0124] S3: The mixing process is:

[0125] First add rubber, mix for 40 seconds, then add zinc oxide ZnO, stearic acid SAD, accelerator 4020, antioxidant RD, microcrystalline wax, plasticizer A; after mixing for 40 seconds, add coupling agent Si69 and precipitated silica; after mixing for 40 seconds, slowly and in multiple times add pyrolysis carbon black and operating oil; after mixing for 40 seconds, lift the plug, and finally mix to 155°C for rubber removal.

[0126] S4: The rubber compound obtained by mixing in S3 is sheeted and vulcanized, and then the performance of the rubber compound is tested.

[0127] (3) Test results

[0128] Table 5 Performance test data of structurally regenerated pyrolytic carbon black

[0129]

[0130]

[0131] Table 6 Performance analysis of rubber composite materials

[0132] Pyrolytic carbon black rubber composites Structural Reconstruction of Pyrolytic Carbon Black Rubber Composites hardness 54.5 65.5 100% fixed stretch 1.82 4.20 200% fixed stretch 5.14 9.85 300% fixed stretch 10.78 18.65 Tensile Strength 22.94 24.89 Elongation at break 476.77 488.28 Tensile product 10933 12153

[0133] From the above experimental data, it can be clearly seen that the performance of the structurally reconstructed pyrolytic carbon black rubber composite material prepared by the present invention far exceeds that of the traditional pyrolytic carbon black rubber composite material, and the 300% elongation reaches 18.65MPa, which meets the performance requirements of the tread rubber of passenger car tires.

[0134] Example 4

[0135] This embodiment provides a device for preparing structurally reconstructed pyrolytic carbon black, such as Figure 1 and 2 As shown, the device includes a continuous feeding extruder I, a device body II, a continuous discharging extruder III, which are connected in sequence, and also includes a frame IV that plays a supporting role.

[0136] The device body II includes a shell 6, on which an electric heating coil for heating and maintaining temperature is installed. A conveying assembly 8 and a protective gas channel 7 are arranged inside the shell 6. The protective gas channel 7 is installed at a position slightly above the middle of the conveying assembly 8. In a specific embodiment, the protective gas channel 7 is installed at a position slightly above 20% of the middle of the conveying assembly 8. Furthermore, a protective gas inlet 2 and a protective gas outlet 3 are also arranged on the shell 6, and the protective gas inlet 2 and the protective gas outlet 3 are respectively connected to the two ends of the protective gas channel 7.

[0137] It can be understood that the conveying component 8 is mainly related to the active carrier material for initiating the reaction (mainly copper foil material in this specific embodiment). Therefore, the conveying component 8 is made of copper foil material, so that the pyrolysis carbon black can achieve the growth of surface functional groups of pyrolysis carbon black under the condition of modification temperature and under the action of the active carrier for initiating the reaction of copper foil.

[0138] The continuous feeding extruder I is fixed on the device body II through a flange, and the continuous feeding extruder I is inserted into the device body II and extends to the top of the conveying assembly 8. The continuous discharging extruder III is fixedly connected to the device body II through a flange, and the continuous discharging extruder III is installed at the bottom of the device body II and forms a 45-degree angle with the shell 6 to facilitate the continuous entry and continuous output of pyrolytic carbon black.

[0139] A transmission assembly 5 and a bearing assembly 4 are fixedly installed on the device body II; a conveying assembly main transmission wheel 9 and a conveying assembly driven transmission wheel 10 are respectively provided at both ends of the conveying assembly 8. The transmission assembly 5 drives the bearing assembly 4 and the conveying assembly main transmission wheel 9 to rotate, and then drives the conveying assembly 8 and the conveying assembly driven transmission wheel 10 to rotate at a uniform speed.

[0140] like Figure 3As shown, in order to ensure that the protective gas does not leak in the device body II, a sealing component 1 needs to be provided at the matching part between the shell 6 and the conveying assembly main drive wheel 9 and the conveying assembly driven drive wheel 10. The sealing assembly 1 is composed of the transmission wheel central shaft 9-1, the sealing dynamic ring 4-1, the sealing ring 4-2, the housing side wall 6-1, the lubricating oil port 6-2, the static sealing upper ring 4-3, the static sealing lower ring 4-4, etc., wherein the sealing dynamic ring 4-1 is a U-shaped structure, interference fit to the corresponding part of the transmission wheel central shaft 9-1, and the sealing working plane of the sealing dynamic ring 4-1 exceeds the working surface of the transmission wheel central shaft 9-1 by 1 to 2 mm; two circular rings are welded at the matching part of the housing side wall 6-1 and the sealing dynamic ring 4-1 to form a precision sealing ring (static sealing upper ring 4-3 and static sealing lower ring 4-4 ​​respectively), wherein the static sealing upper ring 4-3 is 10 mm longer than the static sealing lower ring 4-4; the sealing ring 4-2 is located in the sealing working area between the sealing dynamic ring 4-1 and the static sealing upper ring 4-3 and the static sealing lower ring 4-4. The lubricating oil port 6-2 is passed through the lubricating oil to lubricate the sealing working area.

[0141] The process flow of the pyrolytic carbon black structure reconstruction device provided by the present invention is as follows:

[0142] The pyrolytic carbon black and the added carbon source are uniformly and continuously fed into the conveying assembly 8 in the device body II through the continuous feeding extruder I. The shell 6 in the device body II is equipped with an electric heating coil, so that the device body II always maintains the high temperature required for the pyrolytic carbon black modification process, and under the action of the transmission assembly 5, the bearing assembly 4 and the main transmission wheel 9 of the conveying assembly are driven to rotate, and the main transmission wheel 9 of the conveying assembly rotates to drive the conveying assembly 8 and the driven transmission wheel 10 of the conveying assembly to rotate at a uniform speed. Since the material of the conveying assembly 8 is the copper foil material, which is the active carrier for the initiation reaction required in the pyrolytic carbon black structural reconstruction process, under the action of the added carbon source at high temperature, a new functional group structure grows on the surface of the pyrolytic carbon black. The entire process needs to be carried out in a certain reaction atmosphere. The reaction atmosphere is mainly introduced into the protective gas channel 7 through the protective gas inlet 2. The protective gas channel 7 is installed at a position about 20% above the middle of the conveying assembly 8, so that the protective gas can directly act on the reactive active area of ​​the pyrolytic carbon black, and part of the protective gas is discharged from the protective gas outlet 3. The treated pyrolytic carbon black is continuously output to the outside of the equipment through the continuous discharging extruder III.

[0143] The above description is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, modification, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing structurally reconstructed pyrolytic carbon black, It is characterized in that The preparation method is to fix the added carbon source to the surface of pyrolytic carbon black under certain temperature conditions to form a new pore structure and chemical functional groups, and reshape the structure and surface microchemical environment of pyrolytic carbon black, including the following steps: S1: In a protective gas atmosphere, the temperature is set to 830-980°C, and the added carbon source, pyrolytic carbon black and the initiating reaction active carrier are fully contacted for 5-12 seconds to obtain modified pyrolytic carbon black; S2: treating the modified pyrolytic carbon black at a temperature of 450 to 550° C. with a plasma discharge power of 200 to 400 W for 1 to 3 min; S3: placing the treated modified pyrolytic carbon black in an acid solution with a concentration of 4 to 9 mol / L and soaking for 5 to 15 minutes; S4: Dry; S5: Supercritical carbon dioxide is fully mixed with restructured pyrolytic carbon black and sprayed out with a special nozzle. The strong high-frequency pulsating shear force field formed by the rapid expansion of supercritical carbon dioxide is used to refine the particle size of pyrolytic carbon black, and finally restructured pyrolytic carbon black is obtained; Wherein, the carbon source is any one of gaseous hydrocarbons, high carbon content polymers or thermosetting resins; The initiating reaction active carrier is a copper foil carrier.

2. The preparation method according to claim 1, It is characterized in that The protective gas atmosphere is an inert gas atmosphere, including nitrogen and argon; The gaseous hydrocarbons are selected from gaseous hydrocarbons having a carbon content of more than 90%, including methane; The high carbon content polymer includes any one of polyethylene, polypropylene, polystyrene or a mixture of several of them.

3. The preparation method according to claim 2, It is characterized in that When the carbon source is gaseous hydrocarbon, the gaseous hydrocarbon is continuously introduced at an intake rate of 20 ml / min, and the gaseous hydrocarbon, pyrolytic carbon black and the initiating reaction active carrier are fully contacted for 5 to 10 seconds at a heating rate of 10 to 15 K / min and a final temperature of 900 to 950° C. in an argon protective gas atmosphere; When the carbon source is a high carbon content polymer, the mass ratio of the high carbon content polymer to the pyrolytic carbon black is 1.5 to 2:100, and the pyrolytic carbon black is fully contacted with the decomposition product of the high carbon content polymer and the initiation reaction active carrier for 8 to 12 seconds at a heating rate of 5 to 10 K / min and a final temperature of 830 to 880° C. in an argon protective gas atmosphere; When the carbon source is a thermosetting resin, the mass ratio of the thermosetting resin to the pyrolytic carbon black is 2.5-3.5:

100. In a nitrogen protective gas atmosphere, at a heating rate of 2-5 K / min and a final temperature of 950-980° C., the pyrolytic carbon black is fully contacted with the decomposition product of the thermosetting resin and the initiation reaction active carrier for 5-8 seconds.

4. The preparation method according to claim 3, It is characterized in that In the step S1, the added carbon source is solidified onto the surface of the pyrolytic carbon black to form chemical functional groups; when gaseous hydrocarbons are used as the carbon source, the functional groups are mainly hydroxyl groups; when high carbon content polymers are used as the carbon source, the functional groups are mainly hydroxyl groups and amide groups; when thermosetting resins are used as the carbon source, the functional groups are mainly hydroxyl groups and aromatic groups.

5. The preparation method according to claim 1, It is characterized in that The step S2 partially oxidizes the modified pyrolytic carbon black, that is, the surface carbon source structure of the modified pyrolytic carbon black is strengthened by plasma at a certain temperature; comprising: The modified pyrolytic carbon black is treated at 450°C for 3 min by a plasma discharge power of 200 W; or, The modified pyrolytic carbon black is treated at 500°C for 2 min by a plasma discharge power of 300 W; or, The modified pyrolytic carbon black was treated at 550°C for 1 min by a plasma discharge power of 400 W.

6. The preparation method according to claim 1, It is characterized in that The step S3 is to etch the modified pyrolytic carbon black, wherein the acidic solution is one or both of sulfuric acid and hydrofluoric acid; Among them, under the condition of sulfuric acid: its concentration is 5-9 mol / L, soaking for 10-15 minutes; Under hydrofluoric acid conditions: the concentration is 4-7 mol / L, soak for 5-10 minutes.

7. The restructured pyrolytic carbon black prepared by the preparation method according to any one of claims 1 to 6.

8. The structured reconstructed pyrolytic carbon black according to claim 7, It is characterized in that The structurally reconstructed pyrolytic carbon black is mixed with rubber to prepare a structurally reconstructed pyrolytic carbon black rubber composite material.

9. A device for implementing the preparation method according to any one of claims 1 to 6, It is characterized in that The device comprises a continuous feeding extruder, a device body and a continuous discharging extruder connected in sequence, a transmission assembly and a bearing assembly are fixedly mounted on the device body; the device body comprises a shell, an electric heating coil is mounted on the shell, a conveying assembly and a protective gas channel are arranged inside the shell, the conveying assembly is made of copper foil material, and the protective gas channel is installed at a position slightly above the middle of the conveying assembly; the continuous feeding extruder is inserted into the device body and extends to just above the conveying assembly; a conveying assembly main drive wheel and a conveying assembly driven drive wheel are respectively arranged at both ends of the conveying assembly, the transmission assembly drives the bearing assembly and the conveying assembly main drive wheel to rotate, and then drives the conveying assembly and the conveying assembly driven drive wheel to rotate at a uniform speed; the device is also provided with a sealing assembly.

10. The device according to claim 9, It is characterized in that The continuous discharging extruder is fixedly connected to the device body and forms an angle of 45 degrees with the shell; The shell is also provided with a protective gas inlet and a protective gas outlet, and the protective gas inlet and the protective gas outlet are respectively connected to the two ends of the protective gas channel; The protective gas channel is installed at a position 20% above the middle of the conveying component; A sealing assembly is provided at a position where the shell cooperates with the main transmission wheel of the conveying assembly and the driven transmission wheel of the conveying assembly. The sealing assembly includes a shell side wall, a transmission wheel center axis and a sealing dynamic ring that is interference fit with the transmission wheel center axis. The sealing dynamic ring is a U-shaped structure, and the sealing working plane of the sealing dynamic ring exceeds the working surface of the transmission wheel center axis by 1 to 2 mm. A static sealing upper ring and a static sealing lower ring are provided at a position where the shell side wall and the sealing dynamic ring cooperate. Both the static sealing upper ring and the static sealing lower ring are circular rings. The static sealing upper ring is 10 mm longer than the static sealing lower ring. A sealing ring is provided between the sealing dynamic ring and the static sealing upper ring and the static sealing lower ring. The sealing assembly also includes a lubricating oil port.

Citation Information

Patent Citations

  • Metal material melt extrusion device based on high-frequency induction heating

    CN103894614A

  • Method for catalyzing and thermally cracking automobile waste tires at low temperature into gas and oil

    CN106350092A

  • Carbon coated particles

    CN107709472A

  • Waste tire cracking processing method and system for changing carbon black structure for tire manufacturing

    CN111410975A

  • Method for impurity removal and modification of waste tire pyrolysis carbon black

    CN112375404A