Anticorrosive bactericidal coating for solvent-free epoxy drinking water tank and preparation method of anticorrosive bactericidal coating

Through the combination of solvent-free epoxy coating formula and specific ingredients, the solvent volatility, short service life and harmful substances of existing coatings are solved, and high durability and corrosion resistance are achieved, which meets the ship's drinking water compartment and long-distance transportation. The demand for water distribution projects.

CN118978843APending Publication Date: 2024-11-19DAHAN TECH (CHANGXING) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411035450.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing drinking water tank coatings have solvent volatile, short service life, inability to coat thickly and contain harmful substances, which cannot meet the needs of ship drinking water tanks and long-distance water distribution projects.

Method used

Using solvent-free epoxy coating formulations, including bisphenol A and bisphenol F epoxy resins, modified diluents, titanium dioxide, precipitated barium sulfate, silver ion-doped nanosilica and graphene slurry, through Specific stirring and grinding steps form a mesh structure, improving the durability and corrosion resistance of the coating.

Benefits of technology

Meet environmental protection standards and drinking water safety requirements, extend the service life of the drinking water tank, improve the corrosion resistance of the paint, and resist the corrosion of corrosive substances such as acid and alkali.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a solvent-free epoxy anticorrosive bactericidal coating for a drinking water tank. The solvent-free epoxy anticorrosive bactericidal coating is prepared from the following components in parts by weight: 30-50 parts of a reagent A, 5-15 parts of a reagent B, 5-15 parts of a reactive diluent, 2-5 parts of a non-reactive diluent, 0.5-1.5 parts of a wetting dispersant, 1-3 parts of a rheological additive, 5-20 parts of titanium dioxide, 20-50 parts of precipitated barium sulfate and 1-5 parts of silver ion doped nano silicon dioxide, the preparation method comprises the following steps: preparing the graphene composite material which meets the environmental protection standard and the drinking water safety requirement; durability of the coating is improved, and service life of the drinking water tank is prolonged; the corrosion resistance of the coating is improved, and the coating is resistant to corrosion of corrosive substances such as acid and alkali.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bearing detection, and in particular to a solvent-free epoxy anticorrosive and sterilizing coating for a drinking water tank and a preparation method thereof. Background Art

[0002] At present, most of my country's drinking water tanks, drinking water storage tanks (pools, tanks) and long-distance water distribution facilities are made of carbon steel, aluminum, reinforced concrete, etc. Since the water and drinking products contained or transported (delivered) by these facilities are highly corrosive to the above materials, if their inner walls are not treated with corrosion protection, they will be corroded and damaged, contaminating the drinking water or drinking products. At the same time, harmful substances in the containers will also migrate into the drinking water or drinking products, causing secondary pollution to the drinking water or drinking products, thereby causing waste.

[0003] To this end, the use of coatings for corrosion protection of the inner walls of the above-mentioned facilities is a commonly used, simple, special, economical and effective protection method. This can not only provide an easy-to-clean surface to prevent contamination of drinking water or drinking products by rust, aging residues and external leakage, but also avoid corrosion of container or facility substrates caused by long-term immersion of drinking water or drinking products, and nourishment of microorganisms, so as to ensure that drinking water or drinking products meet the referenced hygiene standards.

[0004] At present, drinking water tank coatings are mainly solvent-based and high-solid coatings. Both types of coatings have the following shortcomings: 1. Solvents evaporate during production and construction; 2. Thick coatings cannot be applied and multiple layers of construction are required; 3. The service life is short and cannot meet the needs of ship drinking water tanks, long-distance water distribution projects and certain closed occasions.

[0005] For this reason, the existing patent CN201310416385.5 is an environmentally friendly epoxy coating for drilling water tanks that can be quickly cured and its manufacturing method. Although it is a solvent-free epoxy, it contains zinc chrome yellow, which does not meet the drinking water hygiene indicators and toxicology indicators. The drying and curing conditions under the thick coating state are not studied, so technical improvements are needed. Summary of the invention

[0006] In view of the deficiencies in the above-mentioned prior art, the object of the present invention is to provide a solvent-free epoxy anticorrosive and sterilizing coating for drinking water tanks.

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks is composed of the following components in weight fractions: 30-50 parts of reagent A, 5-15 parts of reagent B, 5-15 parts of active diluent, 2-5 parts of inactive diluent, 0.5-1.5 parts of wetting dispersant, 1-3 parts of rheological additive, 5-20 parts of titanium dioxide, 20-50 parts of precipitated barium sulfate, 1-5 parts of silver ion-doped nano-silicon dioxide, 1-5 parts of graphene slurry, and 25 parts of alicyclic amine epoxy curing agent.

[0008] Furthermore, the inactive diluent is any one of modified ethyl acetate, dibutyl phthalate or acetone.

[0009] Furthermore, the graphene slurry is preferably a single-layer graphene slurry.

[0010] Furthermore, the active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

[0011] As a preferred embodiment of the present application, the reagent A is bisphenol A epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

[0012] Further, 30-50 parts of reagent A, 5-15 parts of reagent B, 5-15 parts of active diluent, 2-5 parts of inactive diluent, and 0.5-1.5 parts of wetting and dispersing agent are dispersed and ground to obtain component C; 5-20 parts of titanium dioxide, 20-50 parts of precipitated barium sulfate, 1-5 parts of silver ion-doped nano-silicon dioxide, and 1-5 parts of graphene slurry are fully stirred and then ground to obtain component D. The obtained component C, component D and alicyclic amine epoxy curing agent are mixed evenly to obtain the solvent-free epoxy anticorrosive and sterilizing coating for drinking water tanks.

[0013] Furthermore, the stirring rate of the C component is 150-300 rpm, and the stirring time is 10-15 minutes.

[0014] Furthermore, the stirring rate of the D component is 18000 rpm for 20-30 minutes.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: a solvent-free epoxy drinking water tank coating prepared by the present invention 1. meets environmental protection standards and drinking water safety requirements; ② Improve the durability of the coating and extend the service life of the drinking water tank; ③ Improve the corrosion resistance of the coating and resist erosion by corrosive substances such as acids and alkalis. DETAILED DESCRIPTION

[0016] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0017] Example 1 A solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks is composed of the following components in weight fractions: 30 parts of reagent A, 5 parts of reagent B, 5 parts of active diluent, 2 parts of inactive diluent, 0.5 parts of wetting dispersant, 1 part of rheological additive, 5 parts of titanium dioxide, 20 parts of precipitated barium sulfate, 1 part of silver ion-doped nano-silicon dioxide, 1 part of graphene slurry, and 25 parts of alicyclic amine epoxy curing agent.

[0018] The inactive diluent in this embodiment is modified ethyl acetate.

[0019] The graphene slurry is preferably a single-layer graphene slurry.

[0020] The active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

[0021] The reagent A is bisphenol A type epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

[0022] The steps for making the solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks are as follows: 30 parts of bisphenol A epoxy resin reagent, 5 parts of bisphenol F epoxy resin reagent, 5 parts of active diluent, 2 parts of inactive diluent, 0.5 parts of wetting dispersant, and 1 part of rheological additive were dispersed and ground at a stirring rate of 150 rpm for 10 minutes to obtain component C; 5 parts of titanium dioxide, 20 parts of precipitated barium sulfate, 1 part of silver ion-doped nano-silicon dioxide, and 1 part of graphene slurry were fully stirred at a stirring rate of 18,000 rpm for 20 minutes and then ground to obtain component D. The obtained component C, component D and 25 parts of alicyclic amine epoxy curing agent are evenly mixed to obtain the solvent-free epoxy antiseptic and sterilization coating for drinking water tanks.

[0023] Embodiment 2: A solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks is composed of the following components in weight fractions: 30 parts of reagent A, 5 parts of reagent B, 5 parts of active diluent, 2 parts of inactive diluent, 0.5 parts of wetting dispersant, 1 part of rheological additive, 5 parts of titanium dioxide, 20 parts of precipitated barium sulfate, 1 part of silver ion-doped nano-silicon dioxide, 1 part of graphene slurry, and 25 parts of alicyclic amine epoxy curing agent.

[0024] The inactive diluent in this embodiment is dibutyl phthalate.

[0025] The graphene slurry is preferably a single-layer graphene slurry.

[0026] The active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

[0027] The reagent A is bisphenol A type epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

[0028] The steps for making the solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks are as follows: 30 parts of bisphenol A epoxy resin reagent, 5 parts of bisphenol F epoxy resin reagent, 5 parts of active diluent, 2 parts of inactive diluent, 0.5 parts of wetting dispersant, and 1 part of rheological additive were dispersed and ground at a stirring rate of 150 rpm for 10 minutes to obtain component C; 5 parts of titanium dioxide, 20 parts of precipitated barium sulfate, 1 part of silver ion-doped nano-silicon dioxide, and 1 part of graphene slurry were fully stirred at a stirring rate of 18,000 rpm for 20 minutes and then ground to obtain component D. The obtained component C, component D and 25 parts of alicyclic amine epoxy curing agent are evenly mixed to obtain the solvent-free epoxy antiseptic and sterilization coating for drinking water tanks.

[0029] Embodiment 3 A solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks is composed of the following components in weight fractions: 30 parts of reagent A, 5 parts of reagent B, 5 parts of active diluent, 2 parts of inactive diluent, 0.5 parts of wetting dispersant, 1 part of rheological additive, 5 parts of titanium dioxide, 20 parts of precipitated barium sulfate, 1 part of silver ion-doped nano-silicon dioxide, 1 part of graphene slurry, and 25 parts of alicyclic amine epoxy curing agent.

[0030] The inactive diluent in this embodiment is acetone.

[0031] The graphene slurry is preferably a single-layer graphene slurry.

[0032] The active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

[0033] The reagent A is bisphenol A type epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

[0034] The steps for making the solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks are as follows: 30 parts of bisphenol A epoxy resin reagent, 5 parts of bisphenol F epoxy resin reagent, 5 parts of active diluent, 2 parts of inactive diluent, 0.5 parts of wetting dispersant, and 1 part of rheological additive are dispersed and ground at a stirring rate of 150 rpm for 10 minutes to obtain component C; 5 parts of titanium dioxide, 20 parts of precipitated barium sulfate, 1 part of silver ion-doped nano-silicon dioxide, and 1 part of graphene slurry were fully stirred at a stirring rate of 18,000 rpm for 20 minutes and then ground to obtain component D. The obtained component C, component D and 25 parts of alicyclic amine epoxy curing agent are evenly mixed to obtain the solvent-free epoxy antiseptic and sterilization coating for drinking water tanks.

[0035] Embodiment 4 A solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks is composed of the following components in weight fractions: 40 parts of bisphenol A epoxy resin reagent, 10 parts of bisphenol F epoxy resin reagent, 10 parts of active diluent, 3 parts of inactive diluent, 1 part of wetting dispersant, 2 parts of rheological additive, 10 parts of titanium dioxide, 30 parts of precipitated barium sulfate, 3 parts of silver ion-doped nano-silicon dioxide, 3 parts of graphene slurry, and 25 parts of alicyclic amine epoxy curing agent.

[0036] The inactive diluent in this embodiment is modified ethyl acetate.

[0037] The graphene slurry is preferably a single-layer graphene slurry.

[0038] The active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

[0039] The reagent A is bisphenol A type epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

[0040] The steps for making the solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks are as follows: 40 parts of bisphenol A epoxy resin reagent, 10 parts of bisphenol F epoxy resin reagent, 10 parts of active diluent, 3 parts of inactive diluent, 1 part of wetting dispersant, and 2 parts of rheological additive were dispersed and ground at a stirring rate of 150 rpm for 10 minutes to obtain component C; 10 parts of titanium dioxide, 30 parts of precipitated barium sulfate, 3 parts of silver ion-doped nano-silicon dioxide, and 3 parts of graphene slurry were fully stirred at a stirring rate of 18,000 rpm for 20 minutes and then ground to obtain component D. The obtained component C, component D and 25 parts of alicyclic amine epoxy curing agent are evenly mixed to obtain the solvent-free epoxy antiseptic and sterilization coating for drinking water tanks.

[0041] Embodiment 5 A solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks is composed of the following components in weight fractions: 50 parts of bisphenol A epoxy resin reagent, 15 parts of bisphenol F epoxy resin reagent, 15 parts of active diluent, 5 parts of inactive diluent, 1.5 parts of wetting dispersant, 3 parts of rheological additive, 20 parts of titanium dioxide, 50 parts of precipitated barium sulfate, 5 parts of silver ion-doped nano-silicon dioxide, 5 parts of graphene slurry, and 25 parts of alicyclic amine epoxy curing agent.

[0042] The inactive diluent in this embodiment is modified ethyl acetate.

[0043] The graphene slurry is preferably a single-layer graphene slurry.

[0044] The active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

[0045] The reagent A is bisphenol A type epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

[0046] The steps for making the solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks are as follows: Disperse and grind 50 parts of bisphenol A epoxy resin reagent, 15 parts of bisphenol F epoxy resin reagent, 15 parts of active diluent, 5 parts of inactive diluent, 1.5 parts of wetting dispersant, and 3 parts of rheological additive, wherein the stirring rate is 150 rpm for 15 minutes to obtain component C; 20 parts of titanium dioxide, 50 parts of precipitated barium sulfate, 5 parts of silver ion-doped nano-silicon dioxide, and 5 parts of graphene slurry were fully stirred at a stirring rate of 18,000 rpm for 30 minutes and then ground to obtain component D. The obtained component C, component D and 25 parts of alicyclic amine epoxy curing agent are evenly mixed to obtain the solvent-free epoxy antiseptic and sterilization coating for drinking water tanks.

[0047] Embodiment 6 A solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks is composed of the following components in weight fractions: 50 parts of bisphenol A epoxy resin reagent, 15 parts of bisphenol F epoxy resin reagent, 15 parts of active diluent, 5 parts of inactive diluent, 1.5 parts of wetting dispersant, 3 parts of rheological additive, 20 parts of titanium dioxide, 50 parts of precipitated barium sulfate, 5 parts of silver ion-doped nano-silicon dioxide, 5 parts of graphene slurry, and 25 parts of alicyclic amine epoxy curing agent.

[0048] The inactive diluent in this embodiment is modified ethyl acetate.

[0049] The graphene slurry is preferably a single-layer graphene slurry.

[0050] The active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

[0051] The reagent A is bisphenol A type epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

[0052] The steps for making the solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks are as follows: 50 parts of bisphenol A epoxy resin reagent, 15 parts of bisphenol F epoxy resin reagent, 15 parts of active diluent, 5 parts of inactive diluent, 1.5 parts of wetting dispersant, and 3 parts of rheological additive were dispersed and ground at a stirring rate of 150 rpm for 10 minutes to obtain component C; 20 parts of titanium dioxide, 50 parts of precipitated barium sulfate, 5 parts of silver ion-doped nano-silicon dioxide, and 5 parts of graphene slurry were fully stirred at a stirring rate of 18,000 rpm for 20 minutes and then ground to obtain component D. The obtained component C, component D and 25 parts of alicyclic amine epoxy curing agent are evenly mixed to obtain the solvent-free epoxy antiseptic and sterilization coating for drinking water tanks.

[0053] Comparative Example 1 This comparative example is the epoxy coating disclosed in Chinese patent CN112409881A.

[0054] Comparative Example 2 This comparative example is the epoxy coating disclosed in Chinese patent CN112574646A.

[0055] Comparative Example 3 This comparative example is the epoxy coating disclosed in Chinese patent CN112029382A.

[0056] The test results of Examples 1-6 were obtained according to Appendix A of GB5369-2008 "General Technical Specifications for Marine Drinking Water Tank Coatings".

[0057] Table 1 Worst experimental data of this application In Examples 1-6 of the present invention, when bisphenol A epoxy resin reacts with a curing agent, the epoxy groups will open and undergo a cross-linking reaction with the curing agent to form a network structure of molecules, and the overall solvent viscosity is reduced and the fluidity is improved by the blended bisphenol F epoxy resin. At the same time, the graphene slurry used in the present application is combined with the resin matrix, and the amine epoxy curing agent undergoes a cross-linking reaction with the epoxy groups in the epoxy resin to form a network structure of macromolecules to promote the curing of the reagent.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks, characterized in that: The invention is composed of the following components in weight fractions: 30-50 parts of reagent A, 5-15 parts of reagent B, 5-15 parts of active diluent, 2-5 parts of inactive diluent, 0.5-1.5 parts of wetting dispersant, 1-3 parts of rheological additive, 5-20 parts of titanium dioxide, 20-50 parts of precipitated barium sulfate, 1-5 parts of silver ion-doped nano-silicon dioxide, 1-5 parts of graphene slurry and 25 parts of alicyclic amine epoxy curing agent.

2. The solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks according to claim 1, characterized in that: The inactive diluent is any one of modified ethyl acetate, dibutyl phthalate or acetone.

3. The solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks according to claim 2, characterized in that: The graphene slurry is preferably a single-layer graphene slurry.

4. The solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks according to claim 3, characterized in that: The active diluent is 1,4-butanediol diglycidyl ether of Xinyuan Technology, with a viscosity of 10cps / 25°C.

5. The solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks according to claim 1, characterized in that: The reagent A is bisphenol A type epoxy resin; The reagent B is bisphenol F type epoxy resin; The wetting and dispersing agent is a modified silicone polymer, and the rheological additive is polysiloxane.

6. A method for preparing a solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks as described in claims 1-5, characterized in that: Disperse and grind 30-50 parts of reagent A, 5-15 parts of reagent B, 5-15 parts of active diluent, 2-5 parts of inactive diluent, and 0.5-1.5 parts of wetting and dispersing agent to obtain component C; 5-20 parts of titanium dioxide, 20-50 parts of precipitated barium sulfate, 1-5 parts of silver ion-doped nano-silicon dioxide, and 1-5 parts of graphene slurry are fully stirred and then ground to obtain component D. The obtained component C, component D and alicyclic amine epoxy curing agent are mixed evenly to obtain the solvent-free epoxy anticorrosive and sterilizing coating for drinking water tanks.

7. The solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks according to claim 6, characterized in that: The stirring rate of the C component is 150-300 rpm, and the stirring time is 10-15 minutes.

8. The solvent-free epoxy anticorrosive and bactericidal coating for drinking water tanks according to claim 7, characterized in that: The stirring rate of the D component is 18000 rpm for 20-30 minutes.

Citation Information

Patent Citations

  • Anticorrosive coating used for drinking water pipeline and preparation method thereof

    CN105017938A

  • Preparation method for antistatic coating for stainless steel pipe

    CN106221513A

  • Epoxy graphene heavy corrosion-resistant coating, and preparation method and application thereof

    CN107739566A