Anti-condensation and anti-corrosion coating for power grid equipment as well as preparation method and application of anti-condensation and anti-corrosion coating

The anti-condensation and anti-corrosion coating, which combines silicone-modified acrylic resin with microspheres, solves the condensation problem of power grid equipment in complex environments, achieving efficient protection and long-term stable operation.

CN118978852APending Publication Date: 2024-11-19GUANGDONG POWER GRID CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411268461.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing anti-corrosion coatings for power grid equipment require phosphating/chromating treatment before use, which pollutes the environment. Furthermore, they are susceptible to water vapor corrosion in complex and variable outdoor environments, leading to condensation and water droplets, which affects the safe and stable operation of the equipment.

Method used

An anti-condensation and anti-corrosion coating using silicone-modified acrylic resin and microspheres works by blocking heat conduction and slowing down the inward conduction of external low temperatures, forming a highly efficient anti-condensation coating by combining microspheres and curing agents.

Benefits of technology

It achieves excellent anti-condensation, anti-aging, and salt spray resistance for power grid equipment. The coating is easy to disperse evenly, forms a film quickly, extends the service life of the equipment, and saves maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005037903980000051
    Figure BDA0005037903980000051
  • Figure BDA0005037903980000081
    Figure BDA0005037903980000081
  • Figure BDA0005037903980000082
    Figure BDA0005037903980000082
Patent Text Reader

Abstract

The invention provides an anti-condensation and anti-corrosion coating for power grid equipment and a preparation method and application thereof.The anti-condensation and anti-corrosion coating comprises a component A and a component B. The component A comprises, by weight, 40-50 parts of organosilicon modified acrylic resin, 40-45 parts of microspheres and 10-15 parts of pigment, and the component B comprises a curing agent, the anti-condensation and anti-corrosion coating has excellent aging resistance, salt fog resistance and anti-condensation performance, and is suitable for protection of power grid equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to an anti-condensation water anti-corrosion coating for power grid equipment, and a preparation method and application thereof. Background Art

[0002] When the water vapor in the air reaches saturation, it condenses on objects with relatively low temperatures to form condensed water. Power grid equipment is exposed to complex and changeable outdoor environments for a long time and is easily corroded by water vapor, which causes condensation and dew on the internal surfaces of power grid equipment, thus affecting the safe and stable operation of power grid equipment.

[0003] CN107629658A discloses a method for preparing an anticorrosive coating for coastal power equipment. Hydroxy acrylic resin and fluororesin are dissolved in butyl acetate, and then silicon dioxide and titanium nitride are added and stirred and mixed; hexamethylene diisocyanate and dibutyltin dilaurate catalyst are then added and stirred and mixed evenly to prepare an anticorrosive coating for coastal power equipment. By introducing fluororesin into the polyurethane coating, the corrosion resistance, UV resistance and aging resistance of the polyurethane coating are improved. However, the substrate surface needs to be pre-treated before use. The pre-treatment includes cleaning, washing, phosphating / chromating, deionized water washing, drying and other processes. The phosphating / chromating process will produce a large amount of wastewater containing phosphides and chromides, which seriously pollutes the environment.

[0004] Therefore, developing an anti-condensation and anti-corrosion coating with excellent anti-condensation, aging resistance and salt spray resistance is of great significance for the protection of power grid equipment. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method and application thereof. The anti-condensation water anti-corrosion coating has excellent aging resistance, salt spray resistance and anti-condensation water performance, and is suitable for the protection of power grid equipment.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides an anti-condensation water anti-corrosion coating for power grid equipment, wherein the anti-condensation water anti-corrosion coating comprises component A and component B, wherein component A comprises the following components in parts by weight: 40 to 50 parts (e.g., 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, 50 parts, etc.) of organosilicon-modified acrylic resin, 40 to 45 parts (e.g., 40 parts, 40.5 parts, 41 parts, 41.5 parts, 42 parts, 42.5 parts, 43 parts, 43.5 parts, 44 parts, 44.5 parts, 50 parts, etc.) of microspheres, 10 to 15 parts (e.g., 10 parts, 10.5 parts, 11 parts, 11.5 parts, 12 parts, 12.5 parts, 13 parts, 13.5 parts, 14 parts, 14.5 parts, 15 parts, etc.) of pigments, and component B comprises a curing agent.

[0008] Preferably, the mass ratio of component A to component B is 4.5:(0.9-1.1), for example, it can be 4.5:0.9, 4.5:0.95, 4.5:1, 4.5:1.05, 4.5:1.1.

[0009] Preferably, the microspheres include polystyrene microspheres and / or composite silica microspheres.

[0010] Preferably, the particle size of the microspheres is 25 to 50 μm, for example, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.

[0011] Preferably, the pigment includes titanium dioxide and / or barium sulfate powder.

[0012] Preferably, the mesh size of the pigment is 300-500 mesh, for example, 300 mesh, 350 mesh, 400 mesh, 450 mesh, 500 mesh, etc.

[0013] Preferably, the curing agent comprises an HDI trimer curing agent.

[0014] Preferably, the solid content of the organosilicon-modified acrylic resin is 60-70%, for example, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, etc.

[0015] In a second aspect, the present invention provides a method for preparing the anti-condensation water anti-corrosion coating as described in the first aspect, the preparation method comprising the following steps:

[0016] (1) mixing a silicone-modified acrylic resin, microspheres and a pigment to obtain a component A;

[0017] (2) Filter the curing agent to obtain component B.

[0018] Preferably, the rotation speed of the stirring and mixing in step (1) is 1000-2000 r / min, for example, it can be 1000 r / min, 1100 r / min, 1200 r / min, 1300 r / min, 1400 r / min, 1500 r / min, 1600 r / min, 1700 r / min, 1800 r / min, 1900 r / min, 2000 r / min, etc.

[0019] Preferably, the stirring and mixing time in step (1) is 40 to 80 min, for example, 40 min, 50 min, 60 min, 70 min, 80 min, etc.

[0020] Preferably, the stirring and mixing temperature in step (1) is 20-65°C, for example, 20°C, 30°C, 40°C, 50°C, 60°C, 65°C, etc.

[0021] Preferably, the stirring and mixing in step (1) further includes filtering.

[0022] Preferably, the particle size of component A after grinding in step (1) is 20 to 50 μm, for example, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.

[0023] Preferably, the preparation method comprises the following steps:

[0024] (1) mixing the organosilicon-modified acrylic resin, microspheres and pigment at 20 to 65° C. and 1000 to 2000 r / min for 40 to 80 min, and filtering to obtain component A;

[0025] (2) Filter the curing agent using a filter to obtain component B.

[0026] In a third aspect, the present invention provides an anti-condensation water anti-corrosion coating for power grid equipment, wherein the anti-condensation water anti-corrosion coating is prepared from the anti-condensation water anti-corrosion coating as described in the first aspect.

[0027] In a fourth aspect, the present invention provides a method for preparing the anti-condensation water anti-corrosion coating as described in the third aspect, the preparation method comprising evenly mixing component A and component B as described in the first aspect, coating the mixture on the surface of a substrate, and curing the mixture to obtain the anti-condensation water anti-corrosion coating.

[0028] Preferably, the coating further comprises removing rust, grease and dust on the surface of the substrate.

[0029] Preferably, the coating comprises spraying or brushing.

[0030] Preferably, the spraying is performed using a sprayer.

[0031] Preferably, the painting is performed using a brush.

[0032] Preferably, the curing temperature is 5 to 60°C, for example, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, etc.

[0033] In a fifth aspect, the present invention provides an application of the anti-condensation water and anti-corrosion coating as described in the first aspect in preventing condensation water and corrosion on the surface of power grid equipment.

[0034] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The present invention uses organic silicon modified acrylic resin as a film-forming resin, and is matched with microspheres to effectively prevent heat conduction, slow down the speed of external low temperature conduction to the inside, and reduce the formation of condensation on the inner wall of the power grid equipment. The prepared anti-condensation water anti-corrosion coating has excellent anti-condensation water, aging resistance and salt spray resistance, and is suitable for the protection of power grid equipment;

[0037] (2) The anti-condensation water anti-corrosion coating prepared by the present invention is easy to disperse evenly, has a fast film-forming speed, and is easy to construct;

[0038] (3) The anti-condensation water anti-corrosion coating prepared by the present invention can extend the service life of equipment and save maintenance costs. DETAILED DESCRIPTION

[0039] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0040] The raw material information used in the specific examples and comparative examples of the present invention is as follows:

[0041] Silicone modified acrylic resin: Hubei Longsheng Sihai New Materials Co., Ltd., SH-024, solid content 60%;

[0042] Rosin modified acrylic resin: Xiamen Chonghuayuan Chemical Co., Ltd., AR120240, purity 99%;

[0043] Polystyrene microspheres: Suzhou Zhiyi Microsphere Technology Co., Ltd., KBsphere25PS, particle size 25 μm;

[0044] Composite silica microspheres: Suzhou Zhiyi Microsphere Technology Co., Ltd., KBsphere25Si, particle size 25 μm;

[0045] Titanium dioxide: Sichuan Longmang Group, mesh size is 300 mesh;

[0046] Barium sulfate powder: Sichuan Longmang Group, mesh size is 300 mesh;

[0047] HDI trimer curing agent: Wanhua Chemical Group Co., Ltd., WANNATE HT-100, solid content is 100%;

[0048] Isocyanate curing agent: Guangzhou Haoyi New Materials Technology Co., Ltd., CA-2870, 100% solids;

[0049] Carbon steel substrate: Baoshan Iron & Steel Co., Ltd., Q235 steel.

[0050] Examples 1 to 6

[0051] An anti-condensation water anti-corrosion coating for power grid equipment includes component A and component B. The raw materials for preparing the coating are shown in Table 1, wherein the units of each component are all "parts by weight".

[0052] Table 1

[0053]

[0054] The preparation method of the anti-condensation water anti-corrosion coating provided in Examples 1 to 3 comprises the following steps:

[0055] (1) mixing the organosilicon-modified acrylic resin, microspheres and pigment at 50° C. and 1000 r / min for 40 min, and filtering to obtain component A;

[0056] (2) Filter the curing agent using a filter to obtain component B.

[0057] The preparation method of the anti-condensation water anti-corrosion coating provided in Examples 4 to 6 comprises the following steps:

[0058] (1) mixing the organosilicon-modified acrylic resin, microspheres and pigment at 60° C. and 1500 r / min for 60 min, and filtering to obtain component A;

[0059] (2) Filter the curing agent using a filter to obtain component B.

[0060] Example 7

[0061] This embodiment provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof. The only difference between this embodiment and embodiment 1 is that an equal amount of polystyrene microspheres are replaced with alumina microspheres, and other conditions are the same as those in embodiment 1.

[0062] Example 8

[0063] This embodiment provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof. The only difference between this embodiment and Example 1 is that an equal amount of titanium dioxide is replaced by zinc oxide powder, and other conditions are the same as those in Example 1.

[0064] Example 9

[0065] This embodiment provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof. The only difference between this embodiment and Example 1 is that an equal amount of HDI trimer curing agent is replaced by an isocyanate curing agent, and other conditions are the same as those in Example 1.

[0066] Comparative Example 1

[0067] This comparative example provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof. The only difference between the comparative example and Example 1 is that 30 parts of organosilicon-modified acrylic resin are added, and other conditions are the same as those in Example 1.

[0068] Comparative Example 2

[0069] This comparative example provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof. The only difference between the comparative example and Example 1 is that 60 parts of polystyrene microspheres are added, and other conditions are the same as those in Example 1.

[0070] Comparative Example 3

[0071] This comparative example provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof. The only difference between the comparative example and Example 1 is that 30 parts of titanium dioxide are added, and other conditions are the same as those in Example 1.

[0072] Comparative Example 4

[0073] This comparative example provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof, which differs from Example 1 only in that an equal amount of silicone-modified acrylic resin is replaced by rosin-modified acrylic resin, and other conditions are the same as those in Example 1.

[0074] Comparative Example 5

[0075] This comparative example provides an anti-condensation water anti-corrosion coating for power grid equipment and a preparation method thereof, which is different from Example 1 only in that polystyrene microspheres are not added, and other conditions are the same as those in Example 1.

[0076] Performance Testing

[0077] The rust, grease and dust on the surface of the carbon steel substrate were removed, and the components A and B provided by Examples 1 to 9 and Comparative Examples 1 to 5 were mixed evenly in a mass ratio of 4.5:1. The surface of the carbon steel substrate was sprayed at a spray angle of 40° using a spray gun with an air pump pressure of 0.5 MPa and a nozzle aperture of 0.36 mm. The coating was dried and cured at 25°C for 18 hours to obtain an anti-condensation and anti-corrosion coating with a dry film thickness of 150 μm, which was used for bonding strength, salt spray resistance, alkali resistance, acid resistance and anti-condensation performance tests.

[0078] (1) Solid content: measured according to the test method specified in GB / T1725-2007;

[0079] (2) Specific gravity: measured according to the test method specified in GB / T1756;

[0080] (3) Surface drying time and actual drying time: measured according to the test method specified in GB / T1728-1989;

[0081] (4) Adhesion strength: measured according to the pull-off adhesion test method of GB / T5210-2006;

[0082] (5) Salt spray resistance: measured according to the test method specified in GB / T 1771-2007;

[0083] (6) Alkali resistance 10% NaOH: measured according to the test method specified in GB / T 9274-2004;

[0084] (7) Acid resistance 10% H2SO4: measured according to the test method specified in GB / T 9274-2004;

[0085] (8) Hemispherical emissivity (thermal resistance): measured according to the test method specified in HG / T 4341-2012. The test results are shown in Tables 2 and 3:

[0086] Table 2

[0087]

[0088] Table 3

[0089]

[0090]

[0091] From the analysis of the data in Table 2 and Table 3, it can be seen that, taking Examples 1 to 6 as examples, the anti-condensation water anti-corrosion coating of the present invention has excellent adhesion, corrosion resistance and anti-condensation water performance.

[0092] Analysis of Example 1 and Comparative Examples 1 to 3 shows that Comparative Example 1 reduces the amount of silicone-modified acrylic resin, Comparative Example 2 increases the amount of polystyrene microspheres, and Comparative Example 3 increases the amount of titanium dioxide. The corrosion resistance of the coating decreases. This is because the specific content of raw materials is not used, and the bonding strength and density of the coating are reduced.

[0093] From the analysis of Example 1 and Comparative Example 4, it can be seen that in Comparative Example 4, the silicone-modified acrylic resin is replaced by an equal amount of other types of acrylic resins, and the bonding strength of the anti-condensation water anti-corrosion coating is reduced from 5 MPa to 2 MPa, the salt spray resistance is reduced from 30 days without rust to 10 days without rust, and the alkali resistance and acid resistance are both reduced from 15 days without blistering and falling off to 5 days without blistering and falling off.

[0094] From the analysis of Example 1 and Comparative Example 5, it can be seen that in Comparative Example 5, no polystyrene microspheres are added, and the hemispherical emissivity of the anti-condensation water anti-corrosion coating is reduced from 0.9 to 0.5. This is because the polystyrene microspheres can effectively prevent heat conduction, slow down the speed of external low temperature conduction inward, and effectively reduce the formation of condensation on the inner wall.

[0095] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An anti-condensation water anti-corrosion coating for power grid equipment, It is characterized in that The anti-condensation water anti-corrosion coating comprises component A and component B; The component A comprises the following components in parts by weight: 40-50 parts of organosilicon-modified acrylic resin, 40-45 parts of microspheres, and 10-15 parts of pigments; The B component includes a curing agent.

2. The anti-condensation water anti-corrosion coating according to claim 1, It is characterized in that The mass ratio of the component A to the component B is 4.5:(0.9-1.1).

3. The anti-condensation water anti-corrosion coating according to claim 1 or 2, It is characterized in that The microspheres include polystyrene microspheres and / or composite silica microspheres; Preferably, the particle size of the microspheres is 25 to 50 μm; Preferably, the pigment comprises titanium dioxide and / or barium sulfate powder; Preferably, the mesh size of the pigment is 300 to 500 meshes.

4. The anti-condensation water anti-corrosion coating according to any one of claims 1 to 3, It is characterized in that The curing agent includes an HDI trimer curing agent; Preferably, the solid content of the organosilicon-modified acrylic resin is 60-70%.

5. A method for preparing the anti-condensation water anti-corrosion coating according to any one of claims 1 to 4, It is characterized in that The preparation method comprises the following steps: (1) mixing a silicone-modified acrylic resin, microspheres and a pigment to obtain a component A; (2) Filter the curing agent to obtain component B.

6. The preparation method according to claim 5, It is characterized in that The stirring and mixing in step (1) is performed at a speed of 1000 to 2000 r / min; Preferably, the stirring and mixing time in step (1) is 40 to 80 minutes; Preferably, the temperature of the stirring and mixing in step (1) is 20 to 65°C; Preferably, the stirring and mixing in step (1) further comprises filtering; Preferably, the particle size of component A after filtration in step (1) is 20 to 50 μm; Preferably, the filtration in step (2) is performed using a filter.

7. The preparation method according to claim 5 or 6, It is characterized in that The preparation method comprises the following steps: (1) mixing the organosilicon-modified acrylic resin, microspheres and pigment at 20 to 65° C. and 1000 to 2000 r / min for 40 to 80 min, and filtering to obtain component A; (2) Filter the curing agent using a filter to obtain component B. 8.An anti-condensation water anti-corrosion coating for power grid equipment, It is characterized in that The anti-condensation water anti-corrosion coating is prepared from the anti-condensation water anti-corrosion coating according to any one of claims 1 to 4.

9. A method for preparing the anti-condensation water anti-corrosion coating according to claim 8, It is characterized in that The preparation method comprises: mixing the component A and the component B described in any one of claims 1 to 4 evenly, applying the mixture on the surface of a substrate, and curing the mixture to obtain the anti-condensation water anti-corrosion coating; Preferably, the coating further comprises removing rust, grease and dust from the surface of the substrate; Preferably, the coating comprises spraying or brushing.

10. Use of the anti-condensation water and anti-corrosion coating according to any one of claims 1 to 4 in preventing condensation water and corrosion on the surface of power grid equipment.

Citation Information

Patent Citations

  • Fluororesin modified acrylic acid durable heat-insulating anti-corrosive coating

    CN101735699A

  • High-weatherability and heavy-duty anticorrosive acrylic acid modified polysiloxane paint

    CN102766394A

  • Building energy-saving coating and its preparation method

    CN104497741A

  • Heat insulation paint for interior wall and preparation method of heat insulation paint

    CN108467644A

  • High pressure steam impact resistant coating for metal materials and preparation method of coating