Micro-proppant applied to deep reservoir development and preparation method of micro-proppant

Micropropants with particle sizes of 300-600 were prepared by abrasive aid grinding and modified film technology. Combined with ultrasonic screening, the problem of insufficient diffusion of hydraulic fracturing proppants is solved, improving the flow diversion capacity and reducing costs.

CN118978905AInactive Publication Date: 2024-11-19SOUTHWEST PETROLEUM UNIV +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411065533.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the proppant diffusion of hydraulic fracturing is insufficient, and it is impossible to effectively combine to improve the proppant particle size and hydrophobic performance to improve the flow diversion ability.

Method used

By aiding the abrasive abrasives, a microaggregate is formed with a particle size of 300-600, and a modified film is added to its surface to form a hydrophobic outer membrane, and a micropropant is prepared in combination with ultrasonic screening technology.

Benefits of technology

It achieves a smaller particle size and better diffusion performance, improves the flow diversion capacity of hydraulic fracturing, and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978905A_ABST
    Figure CN118978905A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a micro-proppant applied to deep reservoir development, which comprises the following steps: step 1, grinding an aggregate by using a grinding aid in an auxiliary manner to obtain a micro-aggregate, and grinding the aggregate by using a grinding machine; step 2, performing surface modification on the micro-aggregate by using a modifier, namely adding the modified film on the surface of the micro-aggregate, and performing surface modification on the micro-aggregate to obtain a primary micro-proppant; step 3, screening the preliminary micro-proppant obtained in the steps 1-2, and obtaining the micro-proppant with the particle size of 300-600 meshes through screening; compared with a proppant material for improving the flow conductivity by using a micro proppant in the prior art, the proppant material has smaller particle size.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a micro-proppant used for deep reservoir development and a preparation method thereof, and relates to the technical field of micro-proppant. Background Art

[0002] Hydraulic fracturing is an effective means to achieve economic production of shale oil and gas. How to effectively support the hydraulic fractures is the key to ensuring the efficient development of shale oil and gas. Hydraulic fracturing usually pumps proppants of a certain particle size / particle size combination to support the hydraulic fractures that have been opened to maintain the conductivity of the hydraulic fractures. The particle size of the proppant is usually expressed by the "mesh number" of the proppant. The mesh number refers to the number of holes on the screen per square inch. The higher the mesh number, the more holes (the higher the mesh number of the proppant, the smaller its particle size).

[0003] Factors affecting the conductivity of hydraulic fractures include proppant particle size and its diffusivity. Small-sized proppant can be carried into microcracks, and better diffusivity can also make the proppant diffuse evenly in the hydraulic fractures, thereby improving the proppant capacity.

[0004] In the prior art, there are technologies that only increase the aggregate crushing rate to increase the mesh size of the proppant to improve the supporting capacity or only increase the hydrophobicity of the proppant to improve the diffusion performance, but there is no technology that combines the two to improve the supporting capacity.

[0005] SUMMARY OF THE INVENTION

[0006] The purpose of the present invention is to provide a micro-proppant and a preparation method thereof for use in deep reservoir development, so as to solve the problem that there is no high-diffusivity micro-proppant in the prior art.

[0007] In order to achieve the above technical objectives and the above technical effects, the invention is implemented through the following technical solutions:

[0008] A method for preparing a microproppant for deep reservoir development comprises the following steps:

[0009] Step 1, using a grinding aid to assist in grinding the aggregate to obtain the micro-aggregate, wherein the grinding is grinding the aggregate with a grinder;

[0010] Step 2, applying a modifier to perform surface modification on the micro-aggregate, wherein the surface modification is to add the modified film on the surface of the micro-aggregate, and a preliminary micro-proppant is obtained after the surface modification of the micro-aggregate;

[0011] Step 3, screening the preliminary micro-proppant obtained in step 1-2, and obtaining the micro-proppant with a particle size of 300-600 mesh by screening;

[0012] Furthermore, the step 1 is specifically that the grinding aid in the grinder accounts for 0.1% to 0.5% of the granular aggregate for grinding.

[0013] Furthermore, the grinding aid includes 20% to 50% polymeric polyol, 2% to 10% sugar, 2% to 5% calcium lignin sulfonate, 1% to 3% alcohol, 5% to 10% sodium lignin sulfonate, 3% to 5% acetic acid, 0.1% to 1% xanthan gum, 0.2% to 1% hydroxypropyl methylcellulose, and the balance is water.

[0014] Furthermore, the step 2 specifically comprises dissolving 2 parts of ferric nitrate and 2 parts of manganese acetate in 15 parts by weight of water to form a mixed solution, and adding the mixed solution into 100 parts by weight of the micro-aggregate and mixing evenly;

[0015] After mixing evenly, heat and stir until dry;

[0016] After drying, 1 part of borate coupling agent, 2 parts of polyacrylamide, 2 parts of alum, 2 parts of sodium silicate, 2 parts of silicone resin polyether emulsion and 20 parts of water are mixed evenly, and then 4 parts of the mixture are taken and sprayed on the surface of the dried micro-aggregate;

[0017] Furthermore, the polymer polyol is one or a mixture of more than one of polyether polyol, polyester polyol, trimerol, dipropylene glycol, polycaprolactone polyol, polyacrylate polyol, triethanolamine, triisopropanolamine, diethanol monoethanolamine, and diisopropylethanolamine.

[0018] Furthermore, the sugar is one of calcium sugar, sucrose, and molasses, and the alcohol is one of propylene glycol and glycerol.

[0019] Furthermore, the step 3 specifically includes mixing the preliminary micro-proppant with a solvent to prepare a suspension.

[0020] Furthermore, the solvent is a solvent to which any one of sodium chloride, potassium chloride and sodium sulfate is added, and the addition amount is 1% to 35%;

[0021] Furthermore, the suspension is added into a separation device having a sieve, and the mesh size of the sieve is distributed between 100 and 1000 meshes.

[0022] Furthermore, ultrasonic waves are applied to the entire screening system, and the cavitation effect generated by ultrasonic waves in the liquid medium is utilized to enable the micro-proppant carried by the liquid to quickly pass through the screen to complete the screening.

[0023] Another object of the present invention is to disclose a microproppant for use in deep reservoir development, wherein the microproppant is prepared by the above method, comprising:

[0024] The micro-proppant has a particle size of 300-600 meshes, the center of the micro-proppant is micro-aggregate, the micro-aggregate is crushed aggregate, and the outer surface is a modified membrane.

[0025] Furthermore, the aggregate is one or more of metallurgical waste residue, mining waste residue, fuel waste residue, chemical waste residue, industrial solid waste, conventional proppant, and marine particles.

[0026] Beneficial effects:

[0027] The micro-proppant described in the present invention has a solid aggregate core and a hydrophobic modified film wrapped on the outside. The micro-proppant has a particle size of 300-600 meshes. The micro-proppant has good flow conductivity due to its micro-particle size and hydrophobic outer membrane structure. Compared with the proppant material in the prior art that uses micro-proppant to improve flow conductivity, it has a smaller particle size.

[0028] In order to prepare a micro-proppant with a particle size of 300-600 mesh, the present invention uses a specific grinding aid. Under the function of the grinding aid, traditional proppant materials such as quartz sand and other materials can obtain a micro-proppant with a target particle size under a grinder. Compared with the prior art that requires the use of expensive machines to prepare micro-proppant or a complex synthesis method to synthesize micro-proppant, the present invention can not only obtain micro-proppant with a smaller particle size but also reduce costs.

[0029] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a flow chart of the method for preparing a proppant according to an embodiment of the present invention;

[0031] Figure 2 Figure 1 is a diagram of a micro-proppant after dispersion treatment (a) and an untreated micro-proppant (b) in a flat plate experiment described in an embodiment of the present invention;

[0032] Figure 3 Figure 1 shows a micro-proppant (a) subjected to a dispersion treatment and an untreated micro-proppant (b) in a beaker experiment described in an embodiment of the present invention; DETAILED DESCRIPTION

[0033] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the present invention will be described in detail below with reference to the accompanying drawings.

[0034] like Figure 1-3 Shown

[0035] Example 1

[0036] It has been experimentally proven that the discrete support of microproppants can improve the conductivity. The document (the mechanism and selection principle of microproppants for shale oil and gas production increase;

[0037] doi:10.12134 / j.dzykt.2020.03.015) verified the conductivity of discrete supported shale microfractures with 100 mesh and 400 mesh proppants. Combined with the permeability measured in the document, it was 10-200 mD; the corresponding microfracture permeability of 400 mesh proppant was 2-20 mD. It can be seen that microproppants (larger than 200 mesh) have good conductivity.

[0038] In combination with the above research, the applicant has developed a microproppant that specifically realizes the full diffusion function, namely, a microproppant for deep reservoir development described in this embodiment, including: a microproppant with a particle size of 300-600 mesh, the center of the microproppant is micro-aggregate, the micro-aggregate is crushed aggregate, and the outer surface is a modified membrane.

[0039] The micro-aggregate is the main component of the micro-proppant, and the modified membrane is only a thin film attached to the micro-aggregate. It is not difficult to understand that the micro-proppant with a particle size of 300-600 mesh has met the particle size condition for filling in micro-cracks, and on this basis, the modified membrane plays a role in improving diffusivity.

[0040] Combined with the above content, it can be known that the particle size of the micro-aggregate is 300-600 mesh to ensure that the particle size of the micro-proppant is 300-600 mesh. The aggregate needs to meet the physical properties of the proppant, so the aggregate is a solid particle material. Finally, in order to ensure the diffusibility of the invention in this embodiment, the modified membrane is a hydrophobic outer membrane structure.

[0041] After the microproppant is modified, its surface adhesion is a polymer with hydrophilic and hydrophobic segments, which is fixed to the surface of the microproppant through anchoring groups and is not easy to fall off. When the microproppant enters the fracturing, the solvated segments on its surface are dispersed into the fracturing fluid, generating steric hindrance and preventing the microproppant from agglomerating.

[0042] In the prior art, the technology of using the good flow conductivity of micro-proppants to improve the propping efficiency already exists, but for example, (CN 104520531 A) forms proppants through reaction, and uses surfactants to emulsify the proppants to increase the diffusivity, which is uncertain. For example, patents (US 6330916 B1), (US 8461087 B2), (CN 103275694A), (CN 103254888 B), (CN 109957387 A) use proppants prepared in advance, and although the diffusion capacity is certain compared with the proppants formed by reaction, the particles do not reach a particle size level of more than 200 mesh.

[0043] Compared with the prior art, the microproppant with a particle size of 300-600 mesh in the invention of this embodiment has better diffusion performance, and can fill more microcracks than the microproppant with a particle size of less than 200 mesh. Combined with the above theoretical content, it can be known that its flow conductivity is better. In addition, the microproppant described in the invention of this embodiment is wrapped with a modified film, and the microproppant has better diffusion performance under the hydrophobic property of the modified film.

[0044] Example 2

[0045] In order to specifically implement the contents involved in Example 1, this embodiment discloses some specific materials of the micro-proppant structure, and the aggregate is one or more of metallurgical waste slag, mining waste slag, fuel waste slag, chemical waste slag, industrial solid waste, conventional proppants, and marine particles. The aggregates described in this embodiment are all selected from materials classified as brittle proppants.

[0046] In one embodiment, the metallurgical waste slag can be selected from one of blast furnace slag, steel slag, non-ferrous metal slag, ferroalloy slag, and ironmaking furnace slag; in one embodiment, the mining waste slag can be selected from one of stripping waste rock, excavation waste rock, ore dressing waste rock, coal gangue, ore washing waste slag, and various tailings; in one embodiment, the fuel waste slag can be selected from one of coal slag, flue ash, fly ash, and shale ash; in one embodiment, the chemical waste slag can be selected from one of sulfuric acid ore slag, carbide slag, alkali slag, gas furnace slag, phosphorus slag, chromium slag, and boron slag; in one embodiment, the industrial solid waste slag can be selected from one of glass waste slag, ceramic waste slag, and construction waste slag; in one embodiment, the conventional proppant can be selected from one of quartz sand and ceramsite; in one embodiment, the marine particles can be selected from one of marine gravel and mineral debris.

[0047] It can be seen that the aggregates selected by the applicant in this embodiment are all low-cost aggregates. Such a choice can further reduce costs. Compared with the high-diffusion performance micro-proppants formed by reaction in the prior art or the micro-proppants partially synthesized by complex methods, the invention in this embodiment obviously has prospects for mass production.

[0048] Although the aforementioned micro-proppant has a relatively low cost, the brittle proppant is often difficult to crush during actual operation. In the prior art, for example (CN 114289158 A), a new type of grinder is basically used to assist in grinding to achieve a higher crushing rate, which in turn leads to increased costs. In order to solve the aforementioned problem, the applicant carried out Example 3.

[0049] Example 3

[0050] In order to prepare a microproppant for deep reservoir development mentioned in Examples 1-2, in this example, the applicant discloses a specific preparation method of the microproppant described in the above examples. A preparation method of a microproppant for deep reservoir development includes the following steps:

[0051] Step 1, using a grinding aid to assist in grinding the aggregate to obtain the micro-aggregate, wherein the grinding is grinding the aggregate with a grinder.

[0052] Step 2, using a modifier to perform surface modification on the micro-aggregate, wherein the surface modification is to add the modified film on the surface of the micro-aggregate, and the preliminary micro-proppant is obtained after the surface modification of the micro-aggregate.

[0053] Step 3, screening the preliminary micro-proppant obtained in step 1-2, and obtaining the micro-proppant with a particle size of 300-600 mesh by screening.

[0054] Wherein step 1 is grinding the aggregate mentioned in Example 2. When the aggregate is classified as brittle proppant aggregate, the grinding aid in the grinder accounts for 0.1% to 0.5% of the granular aggregate to achieve better grinding results.

[0055] The grinding aid mentioned in step 1 includes 20% to 50% of polymeric polyols, 2% to 10% of sugars, 2% to 5% of calcium lignin sulfonate, 1% to 3% of alcohols, 5% to 10% of sodium lignin sulfonate, 3% to 5% of acetic acid, 0.1% to 1% of xanthan gum, 0.2% to 1% of hydroxypropyl methylcellulose, and the balance is water.

[0056] The polymer polyol is one or a mixture of more than one of polyether polyol, polyester polyol, trimerol, dipropylene glycol, polycaprolactone polyol, polyacrylate polyol, triethanolamine, triisopropanolamine, diethanol monoethanolamine, and diisopropylethanolamine.

[0057] The sugar is one of calcium sugar, sucrose and molasses, and the alcohol is one of propylene glycol and glycerol.

[0058] In one embodiment, the aggregate is tailings or quartz sand and the aforementioned grinding aid is used for comparative experiments. When the grinding aid is not added, the grinding aid is 30% polyether polyol, 5% molasses, 2% calcium lignin sulfonate, 3% ethylene glycol, 8% sodium lignin sulfonate, 3% acetic acid, 0.5% xanthan gum, 0.5% hydroxypropyl methylcellulose, and 48% water, which are mixed evenly.

[0059] To 100 parts of tailings, 0.2% of grinding aid was added.

[0060] The particle size of the micro-aggregate obtained after adding the grinding aid is as follows: when tailings are selected, 300-400 mesh accounts for 14%, 400-500 mesh accounts for 68%, 500-600 mesh accounts for 8%, and other meshes account for 10%; when quartz sand is selected, 300-400 mesh accounts for 72%, 400-500 mesh accounts for 21%, and 500-600 mesh accounts for 3%. Specific embodiment:

[0062] (1) 100 parts of granular materials are selected as tailings;

[0063] (2) then adding no grinding aid to 100 parts of the tailings, and then grinding the tailings to obtain microproppant A, the grinding time being the same as that of Example 1;

[0064] (4) Dissolve 2 parts of ferric nitrate and 2 parts of manganese acetate in 15 parts of water to form a mixed solution to obtain modifier A. Add 1 part of borate coupling agent, 2 parts of polyacrylamide, 2 parts of alum, 2 parts of sodium silicate, and 2 parts of silicone resin polyether emulsion and add 20 parts of water to mix uniformly to obtain modifier B.

[0065] (5) adding 19 parts of modifier A to 100 parts of microproppant A, and then heating and stirring until dry to obtain microproppant B, and then spraying 4 parts of modifier B on the surface of 100 parts of microproppant B, mixing evenly, and drying to obtain microproppant C;

[0066] (6) Dissolve 100 parts of sodium chloride in 1000 parts of liquid to obtain solvent A;

[0067] (7) Add 1000 parts of solvent A to 100 parts of medium-sized micro-proppant C, and then sieve with 300, 400, 500, and 600 mesh sieves; then dry to obtain micro-proppant D with different mesh sizes.

[0068] The screening rate is as follows:

[0069] Table 1 Proppant screening rate

[0070]

[0071]

[0072] That is, the final micro-proppant content within the usable particle size range of grinding without adding grinding aids is greatly reduced. Therefore, it is necessary to add grinding aids. According to the above data, it can be seen that the grinding aids described in this embodiment can effectively improve the grinding efficiency. Compared with the method of using large-scale machine crushing in the prior art, the invention in this embodiment greatly reduces the grinding cost.

[0073] Example 4

[0074] In order to further illustrate the surface modification in step 2 mentioned in Example 3, this example discloses a specific implementation method.

[0075] Specifically, step 2 comprises dissolving 2 parts of ferric nitrate and 2 parts of manganese acetate in 15 parts of water to form a mixed solution, and adding the mixed solution to 100 parts of the micro-aggregate to mix evenly;

[0076] After mixing evenly, heat and stir until dry;

[0077] After drying, 1 part of borate coupling agent, 2 parts of polyacrylamide, 2 parts of alum, 2 parts of sodium silicate, 2 parts of silicone polyether emulsion and 20 parts of water are mixed evenly, and then 4 parts of the mixture are taken and sprayed on the surface of the dried micro-aggregate.

[0078] Combined with the above theoretical content, it can be known that the application of the surface modification technology described in this embodiment can effectively improve the dispersibility, and the applicant further designed an experiment to verify it.

[0079] Microproppant dispersion performance test and verification in this example

[0080] (1) Detection method

[0081] The specific test method for the dispersion performance of micro-proppant is as follows:

[0082] 1) Weigh 5 g of the microproppant and use a beaker to detect its dispersibility, by placing the microproppant in a beaker and observing its dispersion; wherein the preliminary microproppant in sequence number 1 is not subjected to the surface modification treatment.

[0083] 2) Weigh 50 g of the micro-proppant and use a visual plate to test its dispersibility, the specific method is as described in the proppant transport capacity test; wherein the preliminary micro-proppant in sequence number 3 is not subjected to the surface modification treatment.

[0084] (2) Detection plan

[0085] According to the above detection method, the micro-proppant dispersion performance test was carried out, and the specific test scheme is shown in Table 2.

[0086] Table 2 Microproppant dispersion performance test scheme

[0087]

[0088] (3) Microproppant dispersion performance test results

[0089] The experiments in Table 1 were carried out to test the dispersion of the microproppant. The experimental results are as follows: Figure 1 , 2It can be seen that the micro-proppant after dispersibility treatment can be evenly dispersed in the fracturing, while the proppant without addition will aggregate and easily form sand banks.

[0090] Combining the above-mentioned theory with the experimental results, it can be seen that the invention in this embodiment has good diffusion performance, which makes the micro-proppant have good flow conductivity.

[0091] Use 15 parts of water to dissolve 2 parts of ferric nitrate and 2 parts of manganese acetate to form a mixed solution, then add it to 100 parts of micro-proppants, mix evenly, then heat and stir until dry, then add 1 part of borate coupling agent, 2 parts of polyacrylamide, 2 parts of alum, 2 parts of sodium silicate, 2 parts of silicone resin polyether emulsion and 20 parts of water to mix evenly, then take 4 parts of the mixed solution, spray it on the surface of the dried micro-proppants, and then dry to obtain a micro-proppants with good dispersion.

[0092] Microproppants are not easy to disperse in fracturing fluids due to their small particle size and the presence of van der Waals forces in microparticles. This increases the size of microproppants. After adding dispersants to the surface, the polyacrylamide and other materials in it are composed of hydrophilic and hydrophobic segments. When microproppants are added to fracturing, their hydrophobic chains are adsorbed on the surface of the microproppants, while the hydrophilic segments are extended in the aqueous medium, thereby generating sufficient steric hindrance to prevent the microproppants from further aggregating. At the same time, due to the adsorption of iron nitrate and manganese acetate on the surface of microproppants, the microproppants present the same residual charge on the surface, forming a double-layer electrostatic structure to further enhance their dispersibility in water.

[0093] Example 5

[0094] The screening step involved in Example 3 includes mixing the preliminary microproppant with a solvent to prepare a suspension, wherein the solvent is a solvent to which any one of sodium chloride, potassium chloride, and sodium sulfate is added, and the addition amount is 1% to 35%, and the suspension is added to a separation device having a screen, and the mesh number of the screen is distributed between 100 and 1000 meshes.

[0095] In one embodiment, the solvent is salt water. The reason for using salt water is to increase the density of the liquid and enhance the suspension ability of the micro-proppant therein. Specifically, 100 parts of sodium chloride are dissolved in 1000 parts of liquid to obtain solvent A. 1000 parts of solvent A are added to 100 parts of micro-proppant C, and then sieved with 300, 400, 500, and 600 mesh screens; and then dried to obtain the micro-proppant of different mesh sizes.

[0096] In one embodiment, in order to achieve fine and rapid screening and precise control of micro-proppants, ultrasound is applied to the entire screening system, and the cavitation effect generated by ultrasound in the liquid medium is used to make the micro-proppants carried by the liquid pass through the screen quickly. The above method can also reduce the risk of dust pollution and explosion during the screening process.

[0097] The above is only part of the embodiment of the application, and does not limit the application in any form. Any simple modification, equivalent changes and modifications made to the above embodiments still fall within the scope of protection of the technical solution of the application.

Claims

1. A method for preparing a microproppant for deep reservoir development, characterized in that: The following steps are involved: Step 1, using a grinding aid to assist in grinding the aggregate to obtain the micro-aggregate, wherein the grinding is grinding the aggregate with a grinder; Step 2, applying a modifier to perform surface modification on the micro-aggregate, wherein the surface modification is to add the modified film on the surface of the micro-aggregate, and a preliminary micro-proppant is obtained after the surface modification of the micro-aggregate; Step 3, screening the preliminary micro-proppant obtained in step 1-2, and obtaining the micro-proppant with a particle size of 300-600 mesh by screening.

2. The method for preparing a microproppant for deep reservoir development according to claim 1, characterized in that: Specifically, the step 1 comprises grinding the particulate aggregate in a grinding machine with a grinding aid ratio of 0.1% to 0.5%.

3. The method for preparing a microproppant for deep reservoir development according to claim 1, characterized in that: The grinding aid comprises 20% to 50% of polymerized polyol, 2% to 10% of sugar, 2% to 5% of calcium lignin sulfonate, 1% to 3% of alcohol, 5% to 10% of sodium lignin sulfonate, 3% to 5% of acetic acid, 0.1% to 1% of xanthan gum, 0.2% to 1% of hydroxypropyl methylcellulose, and the balance is water.

4. The method for preparing a microproppant for deep reservoir development according to claim 1, characterized in that: Specifically, step 2 comprises dissolving 2 parts of ferric nitrate and 2 parts of manganese acetate in 15 parts by weight of water to form a mixed solution, and adding the mixed solution to 100 parts by weight of the micro-aggregate to mix evenly; After mixing evenly, heat and stir until dry; After drying, 1 part of borate coupling agent, 2 parts of polyacrylamide, 2 parts of alum, 2 parts of sodium silicate, 2 parts of silicone polyether emulsion and 20 parts of water are mixed evenly, and then 4 parts of the mixture are taken and sprayed on the surface of the dried micro-aggregate.

5. The method for preparing a microproppant for deep reservoir development according to claim 3, characterized in that: The polymer polyol is one or a mixture of more than one of polyether polyol, polyester polyol, trimerol, dipropylene glycol, polycaprolactone polyol, polyacrylate polyol, triethanolamine, triisopropanolamine, diethanol monoethanolamine, and diisopropylethanolamine.

6. The method for preparing a microproppant for deep reservoir development according to claim 3, characterized in that: The sugar is one of calcium sugar, sucrose and molasses, and the alcohol is one of propylene glycol and glycerol.

7. The method for preparing a microproppant for deep reservoir development according to claim 3, characterized in that: The solvent is a solvent added with any one of sodium chloride, potassium chloride and sodium sulfate, and the added amount is 1% to 35%.

8. The method for preparing a microproppant for deep reservoir development according to claim 1, characterized in that: The step 3 specifically comprises mixing the preliminary micro-proppant with a solvent to prepare a suspension; The suspension is added into a separation device having a sieve, wherein the mesh number of the sieve is distributed between 100 and 1000 meshes.

9. The method for preparing a microproppant for deep reservoir development according to claim 1, characterized in that: Ultrasonic waves are applied to the entire screening system, and the cavitation effect generated by ultrasonic waves in the liquid medium is used to make the micro-proppant carried by the liquid pass through the screen quickly to complete the screening.

10. A microproppant for use in deep reservoir development, characterized in that: The proppant is prepared by the method of claim 1, comprising: The micro-proppant has a particle size of 300-600 meshes, the center of the micro-proppant is micro-aggregate, the micro-aggregate is crushed aggregate, and the outer surface is a modified membrane.

Citation Information

Patent Citations

  • Easily dispersed modified fly ash adsorbent

    CN105921098A

  • Grinding pad for gallium oxide single crystals and preparation method of grinding pad

    CN106272035A

  • Method for screening micro-nano powder

    CN112642697A

  • Micro-proppant water-based dispersion system and preparation method thereof

    CN115960600A

  • Hydrophobic proppant and preparation method thereof

    US20130225458A1