Method for preparing porous hydrogen storage alloy through metal co-sintering
By aiding the sintering metal powder to form a porous frame of hydrogen storage alloy, the problem of hydrogen storage alloy powder is solved, the anti-powder performance and hydrogen diffusion efficiency are improved, secondary auxiliary materials are avoided, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202411153228.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
AI Technical Summary
Volume changes in hydrogen storage alloys during hydrogen absorption and release lead to powdering, affecting the safety and performance of hydrogen storage containers. The existing solutions can contaminate the alloy parent and reduce the hydrogen diffusion kinetics by adding secondary auxiliary materials.
The sintering metal powder and the hydrogen storage alloy powder are mixed by ball mill to form a porous frame. The sintering neck that binds the hydrogen storage alloy powder is formed by low-temperature sintering, inhibiting powdering and promoting hydrogen diffusion, and avoiding the addition of secondary auxiliary materials.
It significantly improves the anti-powdering performance of the hydrogen storage alloy, enhances the hydrogen diffusion and absorption efficiency, avoids the pollution of the alloy parent body by secondary auxiliary materials, and is easy to operate and suitable for industrial production.
Smart Images

Figure CN118979173A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal hydrogen storage, and in particular to a method for preparing a porous hydrogen storage alloy by metal-assisted sintering. Background Art
[0002] Solid-state hydrogen storage materials, especially hydrogen storage alloys, are important carriers for safe and efficient storage of hydrogen. Further improving the performance of existing hydrogen storage alloy materials has become a hot topic of current research. However, since the volume change of hydrogen storage alloys during hydrogen absorption and release is about 30%, hydrogen storage alloys are very prone to pulverization, resulting in reduced mass and heat transfer performance of the bed, and even local stress concentration that endangers the safety of the hydrogen storage container. Therefore, the anti-pulverization performance of hydrogen storage alloys has always been a difficult problem that needs to be solved urgently. The current mainstream solution is to add secondary auxiliary materials, such as natural expanded graphite, polymers, etc., to form composite hydrogen storage materials to resist the pulverization problem caused by the expansion or contraction process of hydrogen storage alloys. However, the addition of secondary auxiliary materials may contaminate the hydrogen storage alloy matrix on the one hand; on the other hand, it may hinder the diffusion of hydrogen to the surface of the hydrogen storage alloy, thereby reducing the kinetic performance of the hydrogen storage process.
[0003] Therefore, developing porous hydrogen storage alloys with anti-powdering properties without the need for secondary addition of auxiliary materials to avoid contamination of the alloy matrix is a technical problem that needs to be urgently solved in this field. Summary of the invention
[0004] In view of this, the present invention provides a method for preparing porous hydrogen storage alloys by metal-assisted sintering, which does not require secondary addition of auxiliary materials. By using sintering-aid metal powder to connect with a sintering neck to form a framework for binding the hydrogen storage alloy powder, the anti-powdering performance of the hydrogen storage alloy is effectively improved.
[0005] The specific scheme of the present invention is as follows: a method for preparing a porous hydrogen storage alloy by metal-assisted sintering, comprising the following steps: Step 1: Put the raw material hydrogen storage alloy powder, sintering metal powder and pore-forming agent into a ball mill; Step 2, adding solvent and grinding balls, evacuating the vacuum, and then ball milling the mixture to obtain mixed raw material powder; Step 3: Take out the mixed raw material powder and dry it; Step 4: molding the dried mixed raw material powder, calcining to remove the pore-forming agent, and finally sintering to obtain a porous hydrogen storage alloy; Among them, the sintering temperature of the sintering-aiding metal powder is lower than the sintering temperature of the hydrogen storage alloy powder; in the step four, the sintering temperature is greater than or equal to the sintering temperature of the sintering-aiding metal powder and lower than the sintering temperature of the hydrogen storage alloy powder.
[0006] During the long-term exploration and research process, the research and development team of the present invention has tried various solutions, but none of them could solve the pulverization problem, and it is easy to introduce other problems that affect the performance of the hydrogen storage alloy. For example, attempts were made to directly sinter the raw hydrogen storage alloy powder to form a sintering neck during the preparation process, but the result was not only difficult to operate and required a high temperature to be controlled, but also the sintering neck, as a part of the hydrogen storage alloy, still had the possibility of pulverization after hydrogen absorption and expansion, and it would pulverize severely after repeated use, and the anti-pulverization problem still could not be solved. However, after further in-depth exploration, changing ideas, multiple attempts and research, the specific solution of the present invention was obtained, which truly solved the pulverization problem and was easy to operate.
[0007] The present invention adds sintering-aiding metal powder, and mixes it with hydrogen storage alloy powder and pore-forming agent particles by adding solvent wet ball milling, and then sintering. The easily sintered metal powder is used to assist in sintering to form a porous framework that binds the hydrogen storage alloy powder. The hydrogen storage alloy is located in the pores of the framework or is directly connected to the sintering-aiding metal powder by sintering, thereby inhibiting the pulverization and flow of the hydrogen storage alloy, significantly improving the anti-pulverization performance, and the formed porous channels can effectively promote the diffusion and absorption of hydrogen. At the same time, the sintering temperature of the sintering-aiding metal powder used in the present invention is lower than the sintering temperature of the hydrogen storage alloy powder itself. The appropriate sintering temperature is controlled so that at this temperature, the hydrogen storage alloy powder will not self-sinter, but the sintering-aiding metal powder can sinter, and the sintering mainly occurs between the sintering-aiding metal powders, forming a sintering-aiding metal sintering neck, and finally forming a porous framework that binds the hydrogen storage alloy powder through the sintering neck connection.
[0008] The sintering metal powder of the present invention is used as an additive and does not participate in the hydrogen absorption process. It mainly forms a porous framework that binds the hydrogen storage alloy powder through its own sintering, has a large bonding strength, and effectively plays a role in resisting pulverization. At the same time, the sintering temperature is relatively low, and there is no need to introduce the addition of secondary auxiliary materials, which will not pollute the hydrogen storage alloy matrix. The entire preparation method is streamlined, easy to operate, and more suitable for industrial production applications.
[0009] In addition, by adding an appropriate amount of pore-forming agent to increase the porosity, the hydrogen storage alloy's hydrogen absorption expansion space is increased while also increasing the specific surface area of the hydrogen storage alloy, which can effectively improve the mass transfer capacity and hydrogen absorption and desorption efficiency of the hydrogen storage alloy. The added pore-forming agent can be completely removed by low-temperature calcination, avoiding the contamination of the hydrogen storage alloy by secondary auxiliary materials in the current mainstream method and the influence of the hydrogen absorption and desorption kinetics.
[0010] Preferably, the hydrogen storage alloy powder is one or more of titanium-based, vanadium-based, and rare earth-based hydrogen storage alloy powders.
[0011] The method of the invention is suitable for the preparation of hydrogen storage alloys such as titanium series, vanadium series, rare earth series, etc., and has great significance for the practical application of hydrogen storage alloys.
[0012] Preferably, the hydrogen storage alloy powder is one or more of AB5 type hydrogen storage alloy, AB2 type hydrogen storage alloy, and BCC type hydrogen storage alloy.
[0013] Preferably, the sintering aid metal powder is one or more of metal Ni powder, metal Ti powder and metal Cu powder.
[0014] The framework for binding the hydrogen storage alloy powder is formed by sintering metal Ni powder, metal Ti powder and metal Cu powder. The sintering is easy, the framework forming effect is good and the stability is better. Other easily sintered metal alloy powders can also be used as sintering-aiding metal powders.
[0015] Preferably, the pore-forming agent is one or more of ammonium bicarbonate, urea, and PMMA.
[0016] These components of pore-forming agents can significantly increase the porosity and are easy to remove later without leaving any residue, and will not affect the subsequent hydrogen absorption and desorption properties of the hydrogen storage alloy.
[0017] Preferably, in the raw materials, the mass proportion of hydrogen storage alloy powder is 45-85wt%, the mass proportion of sintering aid metal powder is 10-50wt%, and the mass proportion of pore former is 3-10wt%.
[0018] Preferably, the particle size range of the hydrogen storage alloy powder is 50-500 mesh, the particle size range of the sintering aid metal powder is 300-800 mesh, and the particle size range of the pore-forming agent is 200-5000 mesh.
[0019] Preferably, the solvent is anhydrous ethanol, and the amount of the anhydrous ethanol solution added accounts for 15-30% of the total mass of the raw materials.
[0020] Preferably, in the step 2, the mixing is ball-milled after vacuuming, the vacuum is evacuated to less than 10 Pa, grinding balls are added according to a ball-to-material volume ratio of 2:1-4:1, the ball-milling speed is 100-400 r / min, and the ball-milling time is 2-8 h.
[0021] The ball-to-material volume ratio is the volume ratio of grinding balls to raw materials. Grinding balls are added according to the volume of raw materials added to ensure that the raw materials are highly mixed after wet ball milling and the mixed raw material powder is finer.
[0022] Preferably, in step three, the mixed raw material powder is taken out and placed in a vacuum oven for drying at a temperature of 40-80° C. for 4-12 h.
[0023] Preferably, in step 4, the molding pressure is 50-400 MPa.
[0024] Preferably, in step 4, the pore-forming agent is removed by calcination in an inert gas atmosphere furnace, and finally the alloy is sintered in a vacuum furnace to obtain a porous hydrogen storage alloy.
[0025] Preferably, the inert gas is argon or nitrogen, and the pore-forming agent is removed by calcination in an atmosphere furnace, the calcination temperature is 200-500° C., and the calcination time is 1-4 h.
[0026] Preferably, the vacuum degree in the vacuum furnace is ≤10 -3 Pa; the vacuum sintering temperature is 700-1300 ° C, the time is 2-8 h, and the vacuum is maintained unchanged during the sintering process to obtain a porous hydrogen storage alloy.
[0027] Preferably, the ball mill is a nylon ball mill.
[0028] The above technical solution of the present invention includes at least the following beneficial effects: 1. The sintering-aiding metal powder of the present invention is used as an additive, does not participate in the hydrogen absorption process itself, and controls the sintering temperature. It forms a porous framework that binds the hydrogen storage alloy powder through its own sintering, has a high bonding strength, and effectively plays a role in anti-powdering.
[0029] 2. The entire preparation method of the present invention is streamlined and easy to operate. The sintering temperature is relatively low, the energy consumption is low, and there is no need to introduce secondary auxiliary materials as anti-powdering agents. It will not pollute the hydrogen storage alloy matrix and is more suitable for industrial production applications.
[0030] 3. The present invention improves the porosity by adding an appropriate amount of pore-forming agent, thereby effectively improving the mass transfer capacity and hydrogen absorption and desorption efficiency of the hydrogen storage alloy. The added pore-forming agent can be completely removed by low-temperature roasting, which also avoids the contamination of the hydrogen storage alloy by secondary auxiliary materials in the traditional method and the influence of the hydrogen absorption and desorption kinetics. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is an electron microscope scanning image of the porous hydrogen storage alloy in Example 1 of the present invention; Figure 2 The PCT curve of the hydrogen storage and desorption performance of the porous hydrogen storage alloy in Example 1 of the present invention; Figure 3 This is a picture of the porous hydrogen storage alloy obtained in Example 1 of the present invention after three hydrogen storage and desorption cycles; Figure 4 This is a picture of the porous hydrogen storage alloy obtained in Comparative Example 2 of the present invention after three hydrogen storage and desorption cycles. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0033] Example 1 In a mass ratio of 80:15:5, 100-mesh AB5 rare earth hydrogen storage alloy powder, 325-mesh Ti powder and 800-mesh PMMA pore-forming agent particles are loaded into a nylon ball mill, 25wt% of anhydrous ethanol is added as a solvent, and grinding balls are added at a ball-to-material volume ratio of 2:1. After evacuating to less than 10 Pa, the ball mill speed is set to 200 r / min, and the ball mill is milled for 4 hours to mix the materials. Take out the mixed raw material powder, that is, the mixed raw material powder, and place it in a vacuum oven at 50°C for 12 hours to dry. The dried mixed raw material powder is molded under a pressure of 150MPa and pressed into a disc, and then placed in an argon atmosphere furnace at a temperature of 400°C for 4 hours to be calcined to remove the pore-forming agent. Then it is placed in a vacuum furnace and heated to a vacuum degree of 10 -3 The porous hydrogen storage alloy was obtained by sintering at 1050 °C for 2 h under the conditions of 1.5 Pa.
[0034] Example 2 In a mass ratio of 68:26:6, 150-mesh AB5 type hydrogen storage alloy, 800-mesh Cu powder and 900-mesh PMMA pore-forming agent particles are loaded into a nylon ball mill, 25wt% of anhydrous ethanol is added as a solvent, and grinding balls are added at a ball-to-material volume ratio of 3:1. After evacuating to less than 10 Pa, the ball mill speed is set to 250 r / min, and the ball mill is mixed for 6 hours. Take out the mixed raw material powder, that is, the mixed raw material powder, and place it in a vacuum oven at 50°C for 10 hours to dry. The dried mixed raw material powder is molded under a pressure of 150MPa and pressed into a disc, and then placed in an argon atmosphere furnace at a temperature of 420°C for 3 hours to be calcined to remove the pore-forming agent. Then place it in a vacuum furnace and heat it at a vacuum degree of less than 10 -3 The porous hydrogen storage alloy was obtained by sintering at 800 °C for 3 h under pressure of 240 Pa.
[0035] Example 3 In a mass ratio of 55:35:10, 500-mesh AB5 rare earth hydrogen storage alloy, 800-mesh Ni powder and 5000-mesh PMMA pore-forming agent particles were loaded into a nylon ball mill, 30wt% anhydrous ethanol was added as a solvent and grinding balls were added at a ball-to-material volume ratio of 4:1. After evacuating to less than 10 Pa, the ball mill speed was set to 400 r / min, and the ball milling was performed for 8 hours to mix the materials. The mixed raw material powder was taken out and placed in a vacuum oven at 60°C for 10 hours for drying. The dried mixed raw material powder was molded under a pressure of 400MPa and pressed into a disc, which was then placed in a nitrogen atmosphere furnace at a temperature of 500°C for 3 hours to be calcined to remove the pore-forming agent. It was then placed in a vacuum furnace and calcined at a vacuum degree of less than 10 -3 The porous hydrogen storage alloy was obtained by sintering at 1000℃ for 5 h under pressure of 240 Pa.
[0036] Example 4 In a mass ratio of 85:10:5, 50-mesh AB2 titanium-based hydrogen storage alloy powder, 400-mesh Cu powder and 200-mesh ammonium bicarbonate pore-forming agent particles are loaded into a nylon ball mill, 15wt% of anhydrous ethanol is added as a solvent, and grinding balls are added at a ball-to-material volume ratio of 2:1. After evacuating to less than 10 Pa, the ball mill speed is set to 100 r / min, and the ball mill is milled for 2 hours to mix the materials. Take out the mixed raw material powder, that is, the mixed raw material powder, and place it in a vacuum oven at 40°C for 11 hours to dry. The dried mixed raw material powder is molded under a pressure of 50MPa and pressed into a disc, which is then placed in a nitrogen atmosphere furnace at a temperature of 200°C for 4 hours to be calcined to remove the pore-forming agent. Then it is placed in a vacuum furnace and heated to a vacuum degree of 10 -3 The porous hydrogen storage alloy was obtained by sintering at 900 °C for 8 h under pressure of 240 Pa.
[0037] Example 5 In a mass ratio of 45:50:5, 200-mesh BCC vanadium hydrogen storage alloy powder, 300-mesh Ni powder and 2000-mesh urea pore-forming agent particles are loaded into a nylon ball mill, 20wt% anhydrous ethanol is added as a solvent and grinding balls are added at a ball-to-material volume ratio of 3:1. After evacuating to less than 10 Pa, the ball mill speed is set to 400 r / min, and the ball mill is milled for 6 hours to mix the materials. The mixed raw material powder is taken out and placed in a vacuum oven at 80°C for 4 hours for drying. The dried mixed raw material powder is molded under a pressure of 200MPa and pressed into a disc, which is then placed in an argon atmosphere furnace at a temperature of 400°C for 4 hours to be calcined to remove the pore-forming agent. It is then placed in a vacuum furnace and heated to a vacuum degree of 10 -3 The porous hydrogen storage alloy was obtained by sintering at 1200℃ for 4 h under pressure of 240 Pa.
[0038] Comparative Example 1 Compared with Example 1, the only difference is that no sintering-aiding metal powder is added, and the other conditions and steps are consistent with Example 1 to prepare the porous hydrogen storage alloy.
[0039] Ultimately, the experiment failed because the sintering temperature was not high enough to form a qualified hydrogen storage alloy.
[0040] Comparative Example 2 Compared with Example 1, the only difference is that no sintering-aiding metal powder is added, and the sintering temperature is increased to 1300° C. The other conditions and steps are consistent with Example 1 to obtain a hydrogen storage alloy sheet.
[0041] Comparative Example 3 Compared with Example 1, the only difference is that the proportion of added sintering aid metal powder is reduced, that is, the hydrogen storage alloy powder, titanium powder and pore-forming agent particles are loaded into a nylon ball mill at a mass ratio of 90:5:5, and the other conditions and steps are consistent with Example 1 to obtain hydrogen storage alloy sheets.
[0042] The hydrogen storage alloy sheet was placed in an experimental container for anti-powdering performance test: The porous hydrogen storage alloy samples obtained in the above Examples 1-5 and Comparative Examples 1-3 were subjected to three hydrogen storage and dehydrogenation cycle operations under the same environmental conditions, and then the surface and powdering of the samples were observed and recorded, which are summarized in Table 1, and Figure 3 , Figure 4 Shown Porosity test using Archimedes drainage method: The porous hydrogen storage alloy samples obtained in the above examples 1-5 and comparative examples 1-3 were tested for porosity using Archimedes drainage method, and the results were recorded and summarized in the following Tables 1 and Figure 2-3 shown.
[0043]
[0044] From the above table and Figure 1 , Figure 3 , Figure 4 It can be clearly seen that the porous hydrogen storage alloy obtained in the embodiment of the present invention has excellent anti-powdering performance, and the porosity is appropriate, maintained between 30-40%, and can still maintain a good forming state after three hydrogen storage and dehydrogenation cycles. Figure 3 As shown, there are no cracks, only slight edge particle shedding, and excellent anti-powdering performance. Figure 1 As shown, it is the sample of Example 1. It can be clearly seen from the figure that the sintered titanium formed forms an overall frame surrounding the hydrogen storage alloy powder, so that the flow between the hydrogen storage alloy powders is restricted, the anti-powdering performance is improved, and the porosity of the hydrogen storage alloy sample is relatively high, indicating that the addition of sintering aid metal does not affect the porosity of the hydrogen storage alloy.
[0045] In contrast, in Example 2, the hydrogen storage alloy without the addition of sintering metal powder was severely pulverized after three hydrogen storage and dehydrogenation cycles. Figure 4 As shown, there are many obvious cracks on the surface, the edges are severely peeled off, and the anti-powdering performance is poor.
[0046] The present invention also tests the hydrogen storage and desorption performance of the porous hydrogen storage alloy samples obtained in Examples 1-5 using the Sieverts isochoric method.
[0047] The test results show that the samples obtained in Examples 1-5 have good and stable hydrogen storage and release performance. Figure 2 The PCT curve of hydrogen storage and desorption performance of Example 1 is shown. The sample can stably absorb and release hydrogen, achieve high hydrogen absorption performance and release hydrogen more thoroughly, and has excellent hydrogen storage and desorption performance. It also shows again that the porous framework formed by adding sintering metal powder will not pollute the hydrogen storage alloy matrix, will not affect the hydrogen storage and desorption performance of the initial hydrogen storage alloy, and can effectively promote the diffusion and absorption of hydrogen.
[0048] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing porous hydrogen storage alloy by metal-assisted sintering, characterized in that: The following steps are involved: Step 1: Put the raw material hydrogen storage alloy powder, sintering metal powder and pore-forming agent into a ball mill; Step 2, adding solvent and grinding balls, evacuating the vacuum, and then ball milling the mixture to obtain mixed raw material powder; Step 3: Take out the mixed raw material powder and dry it; Step 4: molding the dried mixed raw material powder, calcining to remove the pore-forming agent, and finally sintering to obtain a porous hydrogen storage alloy; Among them, the sintering temperature of the sintering-aiding metal powder is lower than the sintering temperature of the hydrogen storage alloy powder; in the step four, the sintering temperature is greater than or equal to the sintering temperature of the sintering-aiding metal powder and lower than the sintering temperature of the hydrogen storage alloy powder.
2. The method for preparing porous hydrogen storage alloy by metal-assisted sintering according to claim 1, characterized in that: The hydrogen storage alloy powder is one or more of titanium series, vanadium series and rare earth series hydrogen storage alloy powders.
3. The method for preparing porous hydrogen storage alloy by metal-assisted sintering according to claim 1, characterized in that: The sintering aid metal powder is one or more of metal Ni powder, metal Ti powder and metal Cu powder.
4. The method for preparing porous hydrogen storage alloy by metal-assisted sintering according to claim 1, characterized in that: The pore-forming agent is one or more of ammonium bicarbonate, urea and PMMA.
5. A method for preparing a porous hydrogen storage alloy by metal-assisted sintering according to any one of claims 1 to 4, characterized in that: The mass proportion of the hydrogen storage alloy powder in the raw materials is 45-85wt%, the mass proportion of the sintering aid metal powder is 10-50wt%, and the mass proportion of the pore-forming agent is 3-10wt%; The particle size range of the hydrogen storage alloy powder is 50-500 meshes, the particle size range of the sintering aid metal powder is 300-800 meshes, and the particle size range of the pore-forming agent is 200-5000 meshes.
6. The method for preparing porous hydrogen storage alloy by metal-assisted sintering according to claim 1, characterized in that: The solvent is anhydrous ethanol, and the amount of the anhydrous ethanol solution added accounts for 15-30% of the total mass of the raw materials.
7. The method for preparing porous hydrogen storage alloy by metal-assisted sintering according to claim 1, characterized in that: In the step 2, the mixture is ball-milled after vacuuming, the mixture is vacuumed to below 10 Pa, grinding balls are added according to a ball-to-material volume ratio of 2:1-4:1, the speed of ball milling is 100-400 r / min, and the ball milling time is 2-8 h; In the step 3, the mixed raw material powder is taken out and placed in a vacuum oven for drying at a temperature of 40-80°C for 4-12 hours; In the step 4, the molding pressure is 50-400 MPa.
8. A method for preparing porous hydrogen storage alloy by metal-assisted sintering according to any one of claims 1 to 4, 6 to 7, characterized in that: In the step 4, the porous hydrogen storage alloy is obtained by calcining in an inert gas atmosphere furnace to remove the pore-forming agent, and finally sintering in a vacuum furnace.
9. The method for preparing porous hydrogen storage alloy by metal-assisted sintering according to claim 8, characterized in that: The inert gas is argon or nitrogen, and the pore-forming agent is removed by calcination in an atmosphere furnace. The calcination temperature is 200-500° C. and the calcination time is 1-4 h.
10. The method for preparing porous hydrogen storage alloy by metal-assisted sintering according to claim 8, characterized in that: The vacuum degree in the vacuum furnace is ≤10 -3 Pa; the vacuum sintering temperature is 700-1300 ° C, the time is 2-8 h, and the vacuum is maintained unchanged during the sintering process to obtain a porous hydrogen storage alloy.
Citation Information
Patent Citations
Preparation method of high-capacity porous metal alloy block serving as hydrogen storage material
CN102181682A
Porous-based hydrogen storage alloy and preparation method thereof
CN118147475A
Preparation method of porous hydrogen storage alloy
CN118441171A
Manufacture of sintered compact of fe-ti hydrogen storage alloy
JP1989056835A
Hydrogen occluding porous material and its production
JP1993221601A