ODS-FeCrAl alloy and preparation method thereof, nuclear reactor fuel cladding and nuclear reactor

By adding glycerin and/or metal Te to ODS-FeCrAl alloy powder, using its wet film and segregation effects, the problems of large particle size and large engineering volume of alloy powder are solved, refinement and efficient ball milling are achieved, and ODS-FeCrAl is improved. Mechanical properties and sintering sealing properties of the alloy.

CN118979187AInactive Publication Date: 2024-11-19UNIV OF SCI & TECH BEIJING +1

Patent Information

Application Number
CN202411054737.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The powder particle size of ODS-FeCrAl alloy powder is large in mechanical alloying, which requires prolonging the ball milling time. There are many types of process control agents added during the alloying process and the engineering volume is large.

Method used

Glycerol and/or metal Te are used as additives to form a wet film and segregation during ball milling, which reduces the surface energy and adhesion of the powder, improves the fluidity and refinement effect of the powder, and shortens the alloying time.

Benefits of technology

The fine particle size and efficient ball milling of the alloy powder are achieved, which shortens the mechanical alloying time and improves the ball milling efficiency. The average particle size of the obtained ODS-FeCrAl alloy powder is significantly reduced, and the sealing and mechanical properties of the sintering process are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979187A_ABST
    Figure CN118979187A_ABST
Patent Text Reader

Abstract

The invention provides an ODS-FeCrAl alloy and a preparation method thereof, a nuclear reactor fuel cladding and a nuclear reactor, and relates to the field of alloys. The preparation method of the ODS-FeCrAl alloy comprises the following steps: mixing yttrium oxide powder, an additive and FeCrAl alloy powder, and then carrying out ball milling, cooling and drying to obtain the ODS-FeCrAl alloy, the additive comprises glycerol and / or metal Te. According to the preparation method of the ODS-FeCrAl alloy, the surface energy of the powder and the interface energy between the powder particles and the grinding balls are reduced by using the additive, so that adhesion and agglomeration of the powder can be reduced, the energy of the grinding balls can be fully transmitted to the powder, and the ball milling efficiency is improved while the powder is promoted to be refined.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of alloys, and in particular to an ODS-FeCrAl alloy and a preparation method thereof, a nuclear reactor fuel cladding and a nuclear reactor. Background Art

[0002] The stability of nuclear reactor fuel cladding is an important guarantee for the safe operation of nuclear reactions. Currently, nuclear reactors have developed to the third generation, and efforts are being made to develop the fourth generation of nuclear energy systems, which will pay more attention to safety to prevent nuclear leakage from causing harm to humans and the environment. Oxide dispersion strengthened (ODS) FeCrAl alloy has become a nuclear fuel cladding material with great application prospects due to its excellent high temperature mechanical properties and neutron irradiation resistance.

[0003] Studies have shown that the ODS-FeCrAl alloy prepared by mechanical alloying not only retains high-temperature oxidation resistance, but also significantly improves mechanical properties. At the same time, it can reduce the thickness of the cladding tube and significantly reduce neutron loss. The oxide dispersion strengthened alloy is to ball mill the oxide powder and the matrix powder, and then solidify and sinter the obtained alloy powder. Under the same sintering conditions, the powder with smaller particles of the same mass alloy powder has a larger specific surface area, the contact between the particles is closer during the sealing process, and the atomic diffusion capacity of the fine-grained powder is enhanced, thereby promoting the sintering process.

[0004] ODS-FeCrAl alloy prepared by mechanical alloying introduces nano-scale Y2O3, HfO2 and other oxide dispersed phases with smaller size and more uniform dispersion distribution into FeCrAl alloy, thereby significantly improving the high temperature strength of FeCrAl alloy. However, there are the following disadvantages:

[0005] (1) The particle size of ODS-FeCrAl alloy powder prepared by mechanical alloying is relatively large. If smaller powder is to be obtained, the ball milling time needs to be extended;

[0006] (2) During the mechanical alloying process, adding process control agents / surfactant elements can achieve the effect of powder refinement and shortening the mechanical alloying time. However, there are many types of process control agents / surfactant elements to be added, and the concentrations used vary, which results in a large amount of work. Summary of the invention

[0007] The purpose of the present application is to provide an ODS-FeCrAl alloy and a preparation method thereof, a nuclear reactor fuel cladding and a nuclear reactor to solve the above-mentioned problems.

[0008] To achieve the above objectives, this application adopts the following technical solutions:

[0009] A method for preparing an ODS-FeCrAl alloy, comprising:

[0010] Yttrium oxide powder, additives and FeCrAl alloy powder are mixed, and then ball-milled and cooled to obtain the ODS-FeCrAl alloy;

[0011] The additives include glycerol and / or metal Te;

[0012] The amount of the yttrium oxide powder is 0.3%-0.75% of the total mass of the ODS-FeCrAl alloy, the amount of the glycerol added is 1%-4% of the total mass of the ODS-FeCrAl alloy, the amount of the metal Te added is 0.1%-0.4% of the total mass of the ODS-FeCrAl alloy; the balance is the FeCrAl alloy powder;

[0013] The FeCrAl alloy powder comprises, by mass percentage, 12-16% Cr, 3.5-5.5% Al, 0.3-0.5% Ti, 1.0-2.5% W, 0.35-0.55% Zr, and the balance is iron.

[0014] Preferably, the particle size of the yttrium oxide powder is 10-40 nm, and the particle size of the metal Te is 20-60 μm.

[0015] Preferably, the particle size of the FeCrAl alloy powder is 20-60 μm.

[0016] Preferably, the ball milling is performed under an argon atmosphere.

[0017] Preferably, the ball milling medium is a stainless steel ball with a diameter of 5-15 mm.

[0018] Preferably, the ball-to-material mass ratio of the ball mill is (5-20):1.

[0019] Preferably, the ball mill has a rotation speed of 250-400 rpm, runs for 0.75-1.25 h and pauses for 0.25-0.75 h, and the total ball milling time is 35-65 h.

[0020] The present application also provides an ODS-FeCrAl alloy, which is prepared using the ODS-FeCrAl alloy preparation method.

[0021] The present application also provides a nuclear reactor fuel cladding, the raw material of which includes the ODS-FeCrAl alloy.

[0022] The present application also provides a nuclear reactor, comprising the nuclear reactor fuel cladding.

[0023] Compared with the prior art, the beneficial effects of this application include:

[0024] The preparation method of ODS-FeCrAl alloy provided by the present application, the additive includes glycerol and / or metal Te; its mechanism is: during the mechanical alloying process, the powder easily adheres to the grinding ball and the ball mill, resulting in a decrease in the fluidity of the powder. Glycerol has three hydroxyl groups and has a high hydrophilicity. Therefore, during the ball milling process, it is easier to form a wet film on the surface of the powder to improve the dispersibility of the powder, reduce agglomeration, and reduce the adhesion between the powders, thereby improving the fluidity of the powder, and thus improving the powder yield and ball milling efficiency. In addition, due to the high boiling point of glycerol, it can effectively absorb and disperse the heat released during the mechanical alloying process, adjust the temperature in the ball mill, and prevent overheating from causing oxidation of the powder or other heat-induced reactions. The segregation of Te elements at the grain boundaries will hinder the migration of the grain boundaries, thereby inhibiting the growth of grains. During the ball milling process, this effect helps to maintain the fine particle size of the powder. In addition, the addition of Te, a surface active element, can reduce the surface energy of the alloy powder. The reduction in surface energy makes it easier for the powder to generate a new surface during the ball milling process, thereby promoting the refinement of the powder.

[0025] The present application proposes to prepare ODS-FeCrAl alloy powder by mechanical alloying by adding glycerol and / or Te to reduce the surface energy of the powder and the interfacial energy between the powder particles and the grinding balls, thereby reducing the adhesion and agglomeration of the powder, allowing the energy of the grinding balls to be fully transferred to the powder, promoting the refinement of the powder while also improving the ball milling efficiency. The results show that the addition of glycerol as a process control agent results in a smaller particle size of the final alloy powder, with an average particle size of 58.29 μm. By adding Te as a surface active element for mechanical alloying, the final alloy powder obtained has a smaller particle size, with an average particle size of 26.44 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0027] Figure 1 It is a mechanical alloying effect diagram of the embodiment and the comparative example;

[0028] Figure 2 The SEM comparison diagram of the alloys obtained in the embodiment and the comparative example;

[0029] Figure 3 The figure is a comparison diagram of the particle size distribution of the alloys obtained in the embodiment and the comparative example;

[0030] Figure 4 This is a comparison of the powders before and after mechanical alloying for 5 hours and drying after adding 2% glycerol as a process control agent in Example 1. DETAILED DESCRIPTION

[0031] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:

[0032] A method for preparing an ODS-FeCrAl alloy, comprising:

[0033] Yttrium oxide powder, additives and FeCrAl alloy powder are mixed, and then ball-milled and cooled to obtain the ODS-FeCrAl alloy;

[0034] The additives include glycerol and / or metal Te;

[0035] The amount of the yttrium oxide powder is 0.3%-0.75% of the total mass of the ODS-FeCrAl alloy, the amount of the glycerol added is 1%-4% of the total mass of the ODS-FeCrAl alloy, the amount of the metal Te added is 0.1%-0.4% of the total mass of the ODS-FeCrAl alloy; the balance is the FeCrAl alloy powder;

[0036] The FeCrAl alloy powder comprises, by mass percentage, 12-16% Cr, 3.5-5.5% Al, 0.3-0.5% Ti, 1.0-2.5% W, 0.35-0.55% Zr, and the balance is iron.

[0037] Optionally, the amount of the yttrium oxide powder can be 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75% or any value between 0.3% and 0.75% of the total mass of the ODS-FeCrAl alloy; the amount of glycerol added can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or any value between 1% and 4% of the total mass of the ODS-FeCrAl alloy; the amount of metal Te added can be 0.1%, 0.2%, 0.3%, 0.4% or any value between 0.1% and 0.4% of the total mass of the ODS-FeCrAl alloy; the FeC rAl alloy powder, calculated by mass percentage, the Cr content can be 12%, 13%, 14%, 15%, 16% or any value between 12-16%; the Al content can be 3.5%, 4.0%, 4.5%, 5.0%, 5.5% or any value between 3.5-5.5%; the Ti content can be 0.3%, 0.4%, 0.5% or any value between 0.3-0.5%; the W content can be 1.0%, 1.5%, 2.0%, 2.5% or any value between 1.0-2.5%; the Zr content can be 0.35%, 0.40%, 0.45%, 0.50%, 0.55% or any value between 0.35-0.55%; the balance is iron.

[0038] In an optional embodiment, the particle size of the yttrium oxide powder is 10-40 nm, and the particle size of the metal Te is 20-60 μm.

[0039] Optionally, the particle size of the yttrium oxide powder may be 10 nm, 20 nm, 30 nm, 40 nm or any value between 10-40 nm, and the particle size of the metal Te may be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm or any value between 20-60 μm.

[0040] In an optional embodiment, the FeCrAl alloy powder has a particle size of 20-60 μm.

[0041] Optionally, the particle size of the FeCrAl alloy powder may be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm or any value between 20 and 60 μm.

[0042] In an optional embodiment, the ball milling is performed under an argon atmosphere.

[0043] In an optional embodiment, the ball milling medium is a stainless steel ball with a diameter of 5-15 mm.

[0044] In an optional embodiment, the ball-to-material mass ratio of the ball mill is (5-20):1.

[0045] Optionally, the ball-to-material mass ratio of the ball mill can be 5:1, 10:1, 15:1, 20:1 or any value between (5-20):1.

[0046] In an optional embodiment, the ball mill has a rotation speed of 250-400 rpm, runs for 0.75-1.25 h and pauses for 0.25-0.75 h, with a total ball milling time of 35-65 h.

[0047] Optionally, the ball milling speed can be 250 rpm, 300 rpm, 350 rpm, 400 rpm or any value between 250-400 rpm, and the running time can be 0.75 h, 0.8 h, 0.85 h, 0.9 h, 0.95 h, 1.00 h, 1.05 h, 1.10 h, 1.15 h, 1.20 h, 1.25 h or between 0.75-1.25 h. The pause time can be 0.25h, 0.30h, 0.35h, 0.40h, 0.45h, 0.50h, 0.55h, 0.60h, 0.65h, 0.70h, 0.75h or any value between 0.25-0.75h, and the total ball milling time can be 35h, 40h, 45h, 50h, 55h, 60h, 65h or any value between 35-65h.

[0048] Through experimental research, it is known that the optimal addition amount of glycerol is 2%, and the optimal ball milling time is 5h; the optimal addition amount of Te is 0.1%, and the optimal ball milling time is 25h.

[0049] The present application also provides an ODS-FeCrAl alloy, which is prepared using the ODS-FeCrAl alloy preparation method.

[0050] The present application also provides a nuclear reactor fuel cladding, the raw material of which includes the ODS-FeCrAl alloy.

[0051] The present application also provides a nuclear reactor, comprising the nuclear reactor fuel cladding.

[0052] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0053] Example 1

[0054] This embodiment provides an ODS-FeCrAl alloy, and the preparation method thereof comprises the following steps:

[0055] Step 1, weighing 0.476% Y2O3, 2% glycerol, and the balance FeCrAl alloy powder (Cr: 14%, Al: 4.5%, Ti: 0.35%, W: 1.8%, Zr: 0.45%, and the balance iron) according to mass percentage;

[0056] Step 2: Place the weighed raw materials into a ball mill, and select stainless steel balls as grinding balls at a ball-to-material ratio of 10:1 (mass ratio).

[0057] Step 3, vacuuming and filling the assembled ball mill with argon;

[0058] Step 4, high-energy ball milling the raw material at 300 rpm, running for 1 hour and pausing for 0.5 hour, with a total running time of 45 hours;

[0059] Step 5, after the ball mill stops operating, take out the ball mill jar and cool it for 0.5h;

[0060] In step 6, the samples are taken out for XRD and SEM testing.

[0061] Example 2

[0062] This embodiment provides an ODS-FeCrAl alloy, and the preparation method thereof comprises the following steps:

[0063] Step 1, weighing 0.476% Y2O3, 0.1% Te, and the balance FeCrAl alloy powder (Cr: 14%, Al: 4.5%, Ti: 0.35%, W: 1.8%, Zr: 0.45%, and the balance iron) according to mass percentage;

[0064] Step 2, put the weighed raw materials into a ball mill, and select stainless steel balls as grinding balls according to a ball-to-material ratio of 10:1 (mass ratio).

[0065] Step 3, vacuuming and filling the assembled ball mill with argon;

[0066] Step 4, subjecting the raw material to mechanical alloying treatment at 300 rpm, running for 1 hour and pausing for 0.5 hour, with a total running time of 45 hours;

[0067] Step 5, after the ball mill stops operating, take out the ball mill jar and cool it for 0.5h;

[0068] In step 6, the samples are taken out for XRD and SEM testing.

[0069] XRD analysis methods include:

[0070] The mechanically alloyed powder after ball milling was tested using an X-ray diffractometer, with a scanning speed of 10° / min, a range of 15-90°, a scanning step of 0.01°, and each sample was tested for about 10 minutes. The XRD diffraction peak data was used to calculate the grain size and lattice distortion of the mechanically alloyed powder using the Gaussian distribution method.

[0071] SEM analysis methods include:

[0072] Take a small amount of the alloy powder after ball grinding, scan the sample surface with an electron beam, and collect secondary electron information on the sample surface through a detector to obtain the sample surface morphology information.

[0073] Comparative Example 1

[0074] The high-energy ball milling preparation method of the ODS-FeCrAl alloy powder in this comparative example is different from that in Examples 1 and 2 in that: in step (1) of this comparative example, no process control agent is added. The remaining steps are the same.

[0075] Comparative Example 2

[0076] The high-energy ball milling method for preparing ODS-FeCrAl alloy powder in this comparative example is different from that in Examples 1 and 2 in that in step (1) of this comparative example, 2% stearic acid is added as a process control agent (instead of glycerol or Te). The remaining steps are the same.

[0077] Comparative Example 3

[0078] The high-energy ball milling method for preparing ODS-FeCrAl alloy powder in this comparative example is different from that in Examples 1 and 2 in that in step (1) of this comparative example, 2% anhydrous ethanol is added as a process control agent (instead of glycerol or Te). The remaining steps are the same.

[0079] Comparative Example 4

[0080] The high-energy ball milling method for preparing ODS-FeCrAl alloy powder in this comparative example is different from that in Examples 1 and 2 in that in step (1) of this comparative example, 2% carbon tetrachloride is added as a process control agent (instead of glycerol or Te). The remaining steps are the same.

[0081] Table 1 is the relevant effect data of the embodiments and comparative examples, which are as follows:

[0082] Table 1 Effect data

[0083]

[0084]

[0085] Comparative analysis: During the mechanical alloying process, the powder is broken and welded under the frequent impact of the grinding ball, and a large number of defects will be generated inside the powder particles. The appearance of defects destroys the balance between atoms and causes lattice distortion. Therefore, the degree of mechanical alloying of the powder is judged by the size of the lattice distortion. The ODS-FeCrAl alloy powder obtained by Example 1, compared with Comparative Example 1, has a grain size reduced by 7.27%, a lattice distortion increased by 6.52%, an average particle size decreased by 44.46%, and a ball milling time reduced by 85.71%; compared with Comparative Example 2, the grain size is reduced by 35.31%, the lattice distortion increases by 113.04%, the average particle size increases by 20.58%, but the ball milling time is reduced by 66.67%; compared with Comparative Example 3, the grain size increases by 3.21%, the lattice distortion increases by 28.95%, the average particle size decreases by 29.23%, and the ball milling time is reduced by 80%; compared with Comparative Example 4, the grain size is reduced by 0.71%, the lattice distortion increases by 11.36%, the average particle size decreases by 20.29%, and the ball milling time is reduced by 85.71%. The ODS-FeCrAl alloy powder obtained by Example 2 has a grain size reduced by 8.66%, a lattice distortion increased by 26.09%, a mean particle size decreased by 80.17%, and a ball milling time reduced by 28.57% compared with Comparative Example 1; compared with Comparative Example 2, the grain size is reduced by 36.27%, the lattice distortion increases by 152.17%, the mean particle size is reduced by 56.95%, and the ball milling time increases by 66.67%; compared with Comparative Example 3, the grain size is increased by 1.68%, the lattice distortion increases by 52.63%, the mean particle size is reduced by 74.73%, and the ball milling time is the same; compared with Comparative Example 4, the grain size is reduced by 2.19%, the lattice distortion increases by 31.82%, the mean particle size is reduced by 71.54%, and the ball milling time is reduced by 28.57%. In the process of mechanical alloying, 2% glycerol was added as a process control agent, or 0.1% Te was added as a surfactant. Through ball milling, the grain size was reduced to varying degrees, the lattice distortion was increased, and the large particle powder was significantly refined, achieving the powder refinement effect.

[0086] According to Example 1 and Example 2, the parameters are changed to obtain Figures 1 to 3 result.

[0087] Figure 1 The mechanical alloying effects (distribution of yttrium in a single particle) of the embodiments and comparative examples are shown in FIG. 1 , wherein (a) and (b) are ball-milled with 2% glycerol for 5 h, (c) and (d) are ball-milled with 0.1% Te for 25 h, (e) and (f) are ball-milled without adding a process control agent for 35 h, (g) and (h) are ball-milled with 2% stearic acid for 15 h, (i) and (j) are ball-milled with 2% anhydrous ethanol for 25 h, and (k) and (l) are ball-milled with 2% carbon tetrachloride for 35 h;

[0088] Figure 2 The SEM comparison diagram of the alloys obtained in the embodiment and the comparative example is shown in FIG. Figure 3 The figure is a comparison of the particle size distribution of the alloys obtained in the embodiment and the comparative example; wherein (a) is ball milled with 2% glycerol for 5 h, (b) is ball milled with 0.1% Te for 25 h, (c) is ball milled without adding a process control agent for 35 h, (d) is ball milled with 2% stearic acid for 15 h, (e) is ball milled with 2% anhydrous ethanol for 25 h, and (f) is ball milled with 2% carbon tetrachloride for 35 h;

[0089] Figure 4 The following is a comparison of the powders before and after mechanical alloying for 5 hours and drying after adding 2% glycerol as a process control agent in Example 1, wherein (a) is the morphology before drying, and (b) is the morphology after drying. In (a), it can be clearly observed that dirt is attached to the surface of the powder, but no such phenomenon is found after drying, which is the same as the morphology without adding the process control agent. Therefore, in the subsequent hot isostatic pressing 400°C vacuum degassing process of the mechanical alloying powder (the alloy powder prepared in this application is subsequently vacuum degassed at 300-500°C for 20-30h, and then hot isostatic pressing is performed at 1050-1250°C and 120-180MPa for 2-4h to prepare the final ODS-FeCrAl alloy.), the residual glycerol can be removed without adding other steps to remove the residue.

[0090] The method provided in the present application refines the particle size of the alloy powder, shortens the mechanical alloying time, and improves the ball milling efficiency.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing an ODS-FeCrAl alloy, characterized in that: include: Yttrium oxide powder, additives and FeCrAl alloy powder are mixed, and then ball-milled and cooled to obtain the ODS-FeCrAl alloy; The additives include glycerol and / or metal Te; The amount of the yttrium oxide powder is 0.3%-0.75% of the total mass of the ODS-FeCrAl alloy, the amount of the glycerol added is 1%-4% of the total mass of the ODS-FeCrAl alloy, the amount of the metal Te added is 0.1%-0.4% of the total mass of the ODS-FeCrAl alloy; the balance is the FeCrAl alloy powder; The FeCrAl alloy powder comprises, by mass percentage, 12-16% Cr, 3.5-5.5% Al, 0.3-0.5% Ti, 1.0-2.5% W, 0.35-0.55% Zr, and the balance is iron.

2. The method for preparing the ODS-FeCrAl alloy according to claim 1, characterized in that: The particle size of the yttrium oxide powder is 10-40 nm, and the particle size of the metal Te is 20-60 μm.

3. The method for preparing the ODS-FeCrAl alloy according to claim 1, characterized in that: The particle size of the FeCrAl alloy powder is 20-60 μm.

4. The method for preparing the ODS-FeCrAl alloy according to claim 1, characterized in that: The ball milling was performed under an argon atmosphere.

5. The method for preparing the ODS-FeCrAl alloy according to claim 1, characterized in that: The medium of the ball mill is a stainless steel ball with a diameter of 5-15 mm.

6. The method for preparing the ODS-FeCrAl alloy according to claim 1, characterized in that: The ball-to-material mass ratio of the ball mill is (5-20):

1.

7. The method for preparing the ODS-FeCrAl alloy according to any one of claims 1 to 6, characterized in that: The ball mill has a rotation speed of 250-400 rpm, runs for 0.75-1.25 h and pauses for 0.25-0.75 h, and the total ball milling time is 35-65 h.

8. An ODS-FeCrAl alloy, characterized in that: The ODS-FeCrAl alloy is prepared using the preparation method of any one of claims 1 to 7.

9. A nuclear reactor fuel cladding, characterized in that: The raw material comprises the ODS-FeCrAl alloy as claimed in claim 8.

10. A nuclear reactor, characterized in that: Comprising the nuclear reactor fuel cladding as described in claim 9.

Citation Information

Patent Citations

  • Preparation method of FeCrAl based ODS alloy used for nuclear reactor cores

    CN110835716A

  • Preparing method for FeCrAl-based ODS alloy for nuclear reactor jacket

    CN110863148A

  • Method for preparing FeCrAl-based ODS alloy for nuclear reactor accident-resisting fuel element can

    CN110863152A

  • Preparation method of FeCrAl-based ODS alloy material for nuclear reactor

    CN111020346A

  • Preparation method of ball milling process control agent

    CN114410276A

Cited By

  • Dispersion strengthened copper alloy preparation system and method

    CN119772182A

  • Oxide dispersion strengthened iron alloy material

    WO2026168453A1