Thick-wall alloy steel and production method thereof
Through smelting and vacuum treatment, the purity of molten steel is improved, combined with chemical composition optimization and rolling technology, the problems of low-temperature impact toughness and production efficiency of thick-wall alloy steel are solved, and high performance and efficient production of thick-wall alloy steel are achieved.
Patent Information
- Application Number
- CN202411103335.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, when producing thick-wall alloy steel, conventional rolling technology has a great impact on low-temperature impact toughness, and it is difficult to effectively produce steel with a wall thickness of more than 36mm, which fails to meet the needs of larger wall thickness steel.
Improve the purity of the molten steel through smelting, reduce the gas content by vacuum treatment, and produce thick-wall alloy steel by large pressure without controlling rolling. The chemical composition is optimized to control C, Mn, Nb, Ti, V, Mo, Ni, The content of Cu and other elements, combined with electromagnetic stirring and dynamic light pressure technology, adopts conventional rolling technology.
The excellent performance of thick-wall alloy steel is achieved, meeting the requirements of high strength, high toughness and low temperature impact performance, improving production efficiency, and significantly improving the cleanliness and tissue density of the molten steel.
Smart Images

Figure CN118979201A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to alloy steel and a production method thereof, in particular to thick-wall alloy steel and a production method thereof, and belongs to the technical field of iron and steel metallurgy. Background Art
[0002] With the commissioning of thick-gauge continuous casting machines and the mature application of wide and thick plate plant technology, thick-walled alloy steel has been widely used in different fields. Through continuous practice, the use of conventional rolling technology can effectively improve the production efficiency of rolling mills. However, conventional rolling has a greater impact on the impact toughness of the product, especially the low-temperature impact toughness, which puts a great test on the manufacturing process.
[0003] At present, CN101343715B high-strength and high-toughness X70 thick-walled seamless pipeline steel and manufacturing method adopt micro-alloy steel design, which is suitable for the production of thick-walled pipelines with a wall thickness of less than 36mm. The overall structure of the pipe body is uniform, which is a uniform bainite structure, low carbon equivalent, good welding performance, and good low-temperature impact performance. It can fully meet the requirements of deep sea or other cold weather for thick-walled pipelines; 2) The continuous casting, perforation and rolling processes are reasonably formulated to maximize the mechanical properties of the pipeline; 3) The internal spray and external shower quenching method is adopted to greatly improve the hardenability of steel during water quenching, but the rolling in the manufacturing method is unconventional rolling, and the impact performance is affected. In addition, the wall thickness of the pipeline steel does not exceed 36mm, and the production of steel with a larger wall thickness has not been reported; Therefore, developing a thick-walled alloy steel and a production method thereof that can overcome the above defects and adopt conventional rolling and have excellent performance has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0004] The present invention aims at the above-mentioned technical problems, overcomes the shortcomings of the prior art, and provides a thick-walled alloy steel and a production method thereof. The present invention improves the purity of molten steel through smelting, adopts vacuum treatment to reduce the harm of gas content, and produces thick-walled alloy steel by large reduction and uncontrolled rolling, thereby obtaining thick-walled alloy steel with excellent performance.
[0005] In order to solve the above technical problems, the present invention provides a thick-walled alloy steel, the chemical composition of the thick-walled alloy steel is as follows by mass percentage: C: 0.10%-0.18%, Si: 0.10%-0.40%, Mn: 1.00%-1.70%, P≤0.025%, S≤0.020%, Nb: 0.020-0.070%, V: 0.050-0.10%, Ti: 0.008-0.030%, Cr: 0.10-0.30%, Ni≤0.50%, Mo≤0.10%, Cu≤0.30%, Al: 0.015%-0.055%, Ca: 0.0006%-0.0030%, N≤0.0080%, the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%.
[0006] The technical solution further defined in the present invention is: Furthermore, in the aforementioned thick-walled alloy steel, the chemical composition of the thick-walled alloy steel is as follows in percentage by mass: C: 0.10%~0.15%, Si: 0.10%~0.30%, Mn: 1.00%~1.50%, P≤0.020%, S≤0.010%, Nb: 0.020~0.040%, V: 0.050~0.080%, Ti: 0.008~0.020%, Cr: 0.10~0.20%, Ni≤0.50%, Mo≤0.10%, Cu≤0.30%, Al: 0.015%~0.050%, Ca: 0.0006%~0.0020%, N≤0.0080%, and the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%.
[0007] In the aforementioned thick-walled alloy steel, the chemical composition of the thick-walled alloy steel is as follows in percentage by mass: C: 0.13%~0.18%, Si: 0.20%~0.40%, Mn: 1.30%~1.70%, P≤0.015%, S≤0.015%, Nb: 0.040~0.070%, V: 0.080~0.10%, Ti: 0.010~0.030%, Cr: 0.20~0.30%, Ni≤0.50%, Mo≤0.10%, Cu≤0.30%, Al: 0.015%~0.055%, Ca: 0.0010%~0.0030%, N≤0.0080%, the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%.
[0008] The present invention also provides a method for producing thick-walled alloy steel, which specifically comprises the following steps: S1. After desulfurization, smelting is carried out in a smelting furnace, and the tapping temperature of the converter is 1660-1700°C. Alloy, lime and refined slag are added during the tapping process, and aluminum is used for deoxidation; S2. During the alloying process, the bottom blowing argon flow rate is 50-80Nl / min, so that the alloy and slag are melted evenly in 5-10min. After smelting, the molten steel is sent to LF for further deoxidation and alloying; S3, the molten steel is further deoxidized and alloyed in LF, and the degassing and inclusion removal tasks are completed through RH vacuum treatment. After the vacuum is completed, calcium treatment is carried out, and static stirring is performed for 10-15 minutes after calcium treatment; S4, continuous casting superheat 20 ~ 40 ℃, electromagnetic stirring, pulling speed 0.5 ~ 0.7m / min, to ensure dynamic light pressure after straightening section, pressure 8 ~ 12mm; S5. The billet is cast and the billet surface is inspected. The qualified billet is austenitized and heated, and the tapping temperature is 1110-1150 degrees. Conventional rolling is adopted, and the billet is cooled after rolling, and the red-return temperature is 550-650 degrees. S6, the rolled pieces are cooled off the production line, and then cut and marked after 24 hours of cooling; S7, the steel plate is sent to heat treatment for normalizing, the normalizing temperature is 500-600℃; S8. The heat-treated steel plates are piled for cooling, shearing, marking and storage.
[0009] In the aforementioned production method of thick-walled alloy steel, the thickness of the produced thick-walled alloy steel is 100 to 300 mm.
[0010] The beneficial effects of the present invention are: (1) P≤0.025%, S≤0.020%. The high phosphorus and sulfur composition design effectively increases the tapping temperature of the converter smelting, improves the thermodynamic and kinetic conditions of the molten steel, and improves the alloying effect of the molten steel through the large stirring technology electromagnetic stirring after the converter furnace, reduces the smelting pressure of LF, reduces the production of inclusions and the adverse effects of gas content, and is conducive to improving the cleanliness of the molten steel and the quality of the core of the molten steel; C is a traditional strengthening element with the advantages of low cost and good control sensitivity, but a high content also has the disadvantage of negatively affecting the welding performance, mechanical properties and hydrogen-induced cracking (HIC) resistance of steel. In addition, the strength matching relationship between carbon and steel is also particularly important, because the carbon content is proportional to the strength of the steel, but the impact toughness of the steel is significantly reduced, which cannot meet the requirements of high strength and high toughness of the steel. The present invention strictly controls the C content to 0.10% to 0.18%, so that it has good strength and impact toughness, and adopts this medium carbon design to avoid the influence of the peritectic zone on the surface quality; Mn plays a major role in solid solution strengthening in steel. The manganese content in microalloyed structural steel is proportional to its strength, and its impact toughness decreases at a relatively low rate, and does not affect its brittle transition temperature. The Mn content of the present invention is controlled at 1.30% to 1.70% to compensate for the strength loss caused by the reduction in carbon content. Nb is an important microalloying element in this steel. Its mechanism of improving strength is fine grain strengthening and precipitation strengthening. It refines grains, improves strength but does not reduce the low-temperature impact toughness of steel. Through the pinning effect of precipitates, it prevents the grain growth of austenite during the rolling process. However, Nb reduces the high-temperature thermoplasticity of steel and increases the hot cracking tendency of Nb-containing steel ingots. According to the needs of rolled steel pipes, the Nb content is stabilized at 0.020-0.070%; The Ti content is controlled at 0.008-0.030%. Ti can produce strong precipitation strengthening and moderate grain refinement. Titanium has strong chemical activity and is easy to form compounds with C, N, O, and S in steel. In order to reduce the content of solid-dissolved nitrogen in steel, micro-titanium treatment is usually used to fix the nitrogen in the steel. TiN can effectively prevent the growth of austenite grains during heating and play a direct strengthening role. Adding trace amounts of titanium to Nb-containing steel can improve the thermoplasticity of Nb-containing steel and reduce the sensitivity to cracking.
[0011] The V content is controlled at 0.050-0.10%. The strain-induced precipitation of V (C, N) during the rolling process can prevent the recrystallization of deformed austenite and the coarsening of recrystallized austenite grains, but this effect weakens with the decrease of nitrogen content in the steel. Vanadium microalloy steel with ordinary nitrogen content will produce a more obvious precipitation strengthening effect at temperatures below 800°C. The most important role of vanadium is to precipitate a large amount of vanadium in ferrite to produce a strong precipitation strengthening effect, which is very obvious even in normalized steel.
[0012] Mo content is controlled at ≤0.10%. It is the main alloying element of this steel. It expands the austenite phase area, delays the formation of ferrite during the phase transformation from austenite to ferrite, and promotes the formation of bainite. It plays an important role in controlling the phase transformation structure. After adding Mo to the steel, a clear bainite structure can be obtained even at a slower cooling rate. At the same time, due to the phase transformation towards the low temperature direction, the structure can be further refined. In the present invention, Ni≤0.50%, Cu≤0.30%, adding copper can improve the strength and corrosion resistance of the alloy steel, and in order to avoid the hot brittleness caused by the segregation of copper, corresponding Ni is added to reduce the segregation of Cu.
[0013] The present invention meets the tensile strength requirements of steel through reasonable component design, wherein the yield strength reaches 436MPa, the tensile strength reaches 539MPa, the elongation reaches 30%, and the average impact energy (-40°C) reaches 160J.
[0014] (2) In step S2 of the present invention, the argon gas flow rate is controlled within 5-10 minutes. Good thermodynamic and kinetic conditions are conducive to rapid melting of the alloy and slag within 5-10 minutes, thereby improving efficiency.
[0015] (3) The present invention performs RH vacuum treatment after LF alloying, and performs calcium treatment after vacuum treatment. The cleanliness of molten steel is improved by calcium treatment, and the harm of sulfur steel is improved by calcium treatment. A composite inclusion system is produced, and inclusions are fully floated during static stirring and casting processes, thereby improving the cleanliness of molten steel of thick-walled products and improving the core performance requirements of thick-walled alloy wires. (4) The present invention uses a high superheat of 20 to 40 degrees for casting and adopts electromagnetic stirring technology to ensure that the segregation elements are evenly distributed between 1 / 4 and 3 / 4 of the ingot. The more even distribution reduces the adverse effects of the segregation elements on the impact properties.
[0016] (5) High superheat combined with dynamic soft reduction technology. High superheat is conducive to the formation of columnar crystals. The use of large reduction is conducive to improving the ferrite content in the core and ensuring the density of the core structure, which is conducive to low-temperature impact toughness. The thick-walled alloy steel is produced by uncontrolled rolling with large reduction, using conventional rolling technology in the prior art. Conventional rolling technology can effectively improve the production efficiency of the rolling mill.
[0017] (6) The use of 1110-1150 degrees austenitizing technology can reduce the secondary growth of grains during the heating process, increase the density of the core grains of the product, and improve the low-temperature impact performance.
[0018] (7) A reasonable stack cooling system is conducive to the volatilization of the gas content inside the steel plate and the uniformity of the structure. The setting of the tempering temperature promotes the uniformity of the structure, reduces the internal stress of the steel plate, and improves the uniformity of the performance and machinability of the thick-walled alloy steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the microstructure image of the steel plate at 1 / 4 thickness in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] To make the present invention more clear, a thick-walled alloy steel and a production method thereof of the present invention are further described below in conjunction with the accompanying drawings. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Example 1
[0021] The present embodiment provides a thick-walled alloy steel, and the chemical composition of the thick-walled alloy steel is as follows in percentage by mass: C: 0.13%, Si: 0.19%, Mn: 1.36%, P: 0.011%, S: 0.003%, Nb: 0.036%, V: 0.066%, Ti: 0.016%, Cr: 0.19%, Ni: 0.04%, Mo: 0.005%, Cu: 0.030%, Al: 0.035%, Ca: 0.0016%, N: 0.0033%, and the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%.
[0022] The production method of the thick-walled alloy steel specifically comprises the following steps: S1. After desulfurization, smelting is carried out in a smelting furnace, and the tapping temperature of the converter is 1693°C. Alloy, lime and refined slag are added during the tapping process, and aluminum is used for deoxidation; S2, the bottom blowing argon flow rate during the alloying process is 65Nl / min, and the good thermodynamic and kinetic conditions are conducive to the uniform melting of the alloy and slag in 6 minutes. After smelting, the molten steel is sent to LF for further deoxidation and alloying; S3, the molten steel is further deoxidized and alloyed in LF, and the tasks of degassing and removing inclusions are completed through RH vacuum treatment. After the vacuum is completed, calcium treatment is carried out, and static stirring is performed for 13 minutes; S4, continuous casting superheat 33 ℃, electromagnetic stirring, casting speed 0.55m / min, to ensure dynamic soft pressure after straightening section, pressure 10mm; S5. The billet is cast and the billet surface is inspected. The qualified billet is austenitized and heated, and the tapping temperature is 1135 degrees. Conventional rolling in the prior art is adopted, and the billet is cooled after rolling, and the red-returning temperature is 586 degrees. S6, the rolled pieces are cooled off the production line, and then cut and marked after 24 hours of cooling; S7, the steel plate is sent to heat treatment for normalizing, and the normalizing temperature is 553℃; S8. The heat-treated steel plates are piled for cooling, shearing, marking and storage.
[0023] In this embodiment, the thickness of the produced thick-walled alloy steel is 260 mm.
[0024] The microstructure image of the rear wall alloy steel at 1 / 4 thickness is as follows: Figure 1 As shown, the metallographic structure of the steel plate at 1 / 4 is mainly composed of ferrite and pearlite, with dense grains, which ensures the stability of tensile and impact properties. Example 2
[0025] The present embodiment provides a thick-walled alloy steel, the chemical composition of which is as follows by mass percentage: The chemical composition of which is as follows by mass percentage: C: 0.14%, Si: 0.31%, Mn: 1.63%, P: 0.010%, S: 0.006%, Nb: 0.045%, V: 0.093%, Ti: 0.022%, Cr: 0.26%, Ni: 0.02%, Mo: 0.003%, Cu: 0.030%, Al: 0.042%, Ca: 0.0019%, N: 0.0045%, the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%. The production method of the above thick-walled alloy steel specifically includes the following steps: S1. After desulfurization, smelting is carried out in a smelting furnace, the tapping temperature of the converter is 1668°C, alloy, lime and refined slag are added during the tapping process, and aluminum is used for deoxidation; S2, During the alloying process, the bottom blowing argon flow rate is 70Nl / min. Good thermodynamic and kinetic conditions are conducive to the uniform melting of alloy and slag in 8 minutes. After smelting, the molten steel is sent to LF for further deoxidation and alloying; S3, the molten steel is further deoxidized and alloyed in LF, and the degassing and inclusion removal tasks are completed through RH vacuum treatment. After the vacuum is completed, calcium treatment is carried out, and static stirring is performed for 12 minutes after calcium treatment; S4, continuous casting superheat 38 ℃, electromagnetic stirring, casting speed 0.60m / min, to ensure dynamic soft pressure after straightening section, pressure 12mm; S5. The billet is cast and the billet surface is inspected. The qualified billet is austenitized and heated, and the tapping temperature is 1141 degrees. Conventional rolling in the prior art is adopted, and the billet is cooled after rolling, and the red-returning temperature is 630 degrees. S6, the rolled pieces are cooled off the production line, and then cut and marked after 24 hours of cooling; S7, the steel plate is sent to heat treatment for normalizing, and the normalizing temperature is 589℃; S8. The heat-treated steel plates are piled for cooling, shearing, marking and storage.
[0026] In this embodiment, the thickness of the produced thick-walled alloy steel is 120 mm.
[0027] The mechanical properties of the steel plates produced in Examples 1 and 2 were tested, and the data are shown in Tables 1 and 2. Table 1 Transverse and longitudinal tensile properties Example direction Yield strength (MPa) Tensile strength (MPa) Elongation (%) Yield-to-strength ratio Example 1 Horizontal 389 465 29 84 Example 2 Horizontal 436 539 30 81 Table 2 -40°C low temperature impact toughness Example Impact energy single value (-40℃) Impact energy single value (-40℃) Impact energy single value (-40℃) Impact energy average (-40℃) Example 1 169J 172J 139J 160J Example 2 129J 181J 156J 155J Cold bending Transverse specimen, 180 degree bend, 3a, qualified.
[0028] As can be seen from Table 1 and Table 2, the present invention improves the purity of molten steel through smelting, adopts vacuum treatment to reduce the harm of gas content, and adopts a large reduction and uncontrolled rolling method to produce thick-walled alloy steel, thereby obtaining a thick-walled alloy steel product with excellent performance, which meets the Q355-Q420 level in the GB / T 1591 standard, and the tensile properties, Charpy impact toughness, and cold bending requirements meet the requirements of the GB / T1591 standard. According to the product performance requirements, the present invention conducts in-depth research through smelting process and casting method of casting machine, applies reasonable composition design combined with optimization process method, and realizes the method that conventional rolling technology meets the low-temperature impact toughness of thick-walled alloy steel. While reducing production costs and improving production efficiency, it meets the customer's usage requirements and successfully develops thick-gauge alloy steel plates.
[0029] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.
Claims
1. A thick-walled alloy steel, characterized in that: The chemical composition of the thick-walled alloy steel is as follows in percentage by mass: C: 0.10%~0.18%, Si: 0.10%~0.40%, Mn: 1.00%~1.70%, P≤0.025%, S≤0.020%, Nb: 0.020~0.070%, V: 0.050~0.10%, Ti: 0.008~0.030%, Cr: 0.10~0.30%, Ni≤0.50%, Mo≤0.10%, Cu≤0.30%, Al: 0.015%~0.055%, Ca: 0.0006%~0.0030%, N≤0.0080%, the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%.
2. The thick-walled alloy steel according to claim 1, characterized in that: The chemical composition of the thick-walled alloy steel is as follows in percentage by mass: C: 0.10%-0.15%, Si: 0.10%-0.30%, Mn: 1.00%-1.50%, P≤0.020%, S≤0.010%, Nb: 0.020-0.040%, V: 0.050-0.080%, Ti: 0.008-0.020%, Cr: 0.10-0.20%, Ni≤0.50%, Mo≤0.10%, Cu≤0.30%, Al: 0.015%-0.050%, Ca: 0.0006%-0.0020%, N≤0.0080%, the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%.
3. The thick-walled alloy steel according to claim 1, characterized in that: The chemical composition of the thick-walled alloy steel is as follows in percentage by mass: C: 0.13%~0.18%, Si: 0.20%~0.40%, Mn: 1.30%~1.70%, P≤0.015%, S≤0.015%, Nb: 0.040~0.070%, V: 0.080~0.10%, Ti: 0.010~0.030%, Cr: 0.20~0.30%, Ni≤0.50%, Mo≤0.10%, Cu≤0.30%, Al: 0.015%~0.055%, Ca: 0.0010%~0.0030%, N≤0.0080%, the remainder is Fe and unavoidable impurities, and the sum of the above components is 100%.
4. A method for producing thick-walled alloy steel according to any one of claims 1 to 3, characterized in that: The specific steps include: S1. After desulfurization, smelting is carried out in a smelting furnace, and the tapping temperature of the converter is 1660-1700°C. Alloy, lime and refined slag are added during the tapping process, and aluminum is used for deoxidation; S2. During the alloying process, the bottom blowing argon flow rate is 50-80Nl / min, so that the alloy and slag are melted evenly in 5-10min. After smelting, the molten steel is sent to LF for further deoxidation and alloying; S3, the molten steel is further deoxidized and alloyed in LF, and the degassing and inclusion removal tasks are completed through RH vacuum treatment. After the vacuum is completed, calcium treatment is carried out, and static stirring is performed for 10-15 minutes after calcium treatment; S4, continuous casting superheat 20 ~ 40 ℃, electromagnetic stirring, pulling speed 0.5 ~ 0.7m / min, to ensure dynamic light pressure after straightening section, pressure 8 ~ 12mm; S5. The billet is cast and the billet surface is inspected. The qualified billet is austenitized and heated, and the tapping temperature is 1110-1150 degrees. Conventional rolling is adopted, and the billet is cooled after rolling, and the red-returning temperature is 550-650 degrees. S6, the rolled pieces are cooled off the production line, and then cut and marked after 24 hours of cooling; S7, the steel plate is sent to heat treatment for normalizing, the normalizing temperature is 500-600℃; S8. The heat-treated steel plates are piled for cooling, shearing, marking and storage.
5. The method for producing thick-walled alloy steel according to claim 4, characterized in that: The thickness of the thick-walled alloy steel produced is 100 to 300 mm.