Hot rolled steel for metal cold cutting circular saw blade base body and production method

By optimizing the production process of hot-rolled plates, the problem of insufficient matching of steel for metal cold-cut circular saw blades is solved, and the refinement and uniformization of metallographic structure is achieved, cutting accuracy and high-speed cutting ability are improved, and the cutting accuracy and high-speed cutting ability are extended. Lifetime of saw blade.

CN118979202APending Publication Date: 2024-11-19武汉钢铁有限公司

Patent Information

Application Number
CN202411069211.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing steel for metal cold-cut circular saw blades has insufficient strength and toughness matching, resulting in cracking, poor cutting accuracy, poor fatigue resistance and high temperature performance, and cannot meet the requirements of high precision and high speed cutting.

Method used

By optimizing the production process of hot-rolled plates, controlling chemical composition and process parameters, including converter smelting, LF furnace refining, RH vacuum treatment, heating, rolling and cooling, improving the cleanliness of steel and refining metallographic structure. Uniformity ensures low inclusions, control of PSN and decarbonization layers in the appropriate range, and the spacing between pearlite sheets is between 150-200 nm.

Benefits of technology

It significantly improves the forming accuracy and pass rate of metal cold-cut circular saw blades, reduces the inclusion level and uneven stress distribution, extends the service life of the saw blades, and is suitable for high-speed continuous cutting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979202A_ABST
    Figure CN118979202A_ABST
Patent Text Reader

Abstract

The invention discloses hot rolled steel for a metal cold cutting circular saw blade base body. The hot rolled steel comprises, by weight, 0.56%-0.86% of C, 0.10%-0.50% of Si, 0.20%-1.00% of Mn, 0.20%-1.00% of Cr, 0.40%-1.50% of Ni, 0.01%-0.30% of Mo, 0.01%-0.30% of V, smaller than or equal to 0.010% of P, smaller than or equal to 0.003% of S, smaller than or equal to 0.002% of N and the balance Fe. The production method comprises the following steps: smelting in a converter, and carrying out LF external refining; performing RH vacuum treatment; after casting into a blank, heating the casting blank; performing conventional rough rolling after high-pressure water descaling; finish rolling; front-section cooling is adopted; performing coiling; and reserving. Through optimization of a hot-rolled plate production process, the cleanliness of steel can be improved, inclusions are smaller than or equal to 0.5 grade, all the inclusions are spherical D-type inclusions, the sum of PSN is smaller than 0.015%, a decarburized layer is controlled to be in a hot rolling state of 30-40 microns, the surface of a finished product has no decarburization characteristic, meanwhile, a metallographic structure is refined and homogenized, the pearlite sheet spacing is 150-200 nm, and the thickness of the finished product is 10-20 microns. Products produced by the prepared cold cutting saw are accurate in formability, and the percent of pass is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to tool steel and a production method, in particular to hot-rolled steel for a metal cold-cutting circular saw blade substrate and a production method. Background Art

[0002] Metal cold cutting circular saw blades have the characteristics of high cutting efficiency, good cross-section quality and high precision. They are widely used in the production processes of cutting and cutting metal materials such as profiles and bars, and are the main cutting equipment for machinery manufacturing, profiles and bars. Cold cutting saw blades are generally produced with saw blade steels such as 65Mn, 75Cr1, and 8CrV, and have very high requirements for material strength, uniformity, fatigue resistance, and high temperature resistance. In the prior art, the main problems of the steel used for metal cold cutting circular saw blades are poor matching of strength and toughness, and the pursuit of high strength is prone to cracking, and the production yield is low; the material uniformity is poor, the stress fluctuation is greater than 50MPa, and it is easy to deform during use, resulting in poor cutting accuracy; the fatigue resistance is poor, which is manifested in the short user use time, early fracture, and the number of cutting times is less than 10,000 times (cutting medium carbon steel bars with a diameter of 60mm); the high temperature performance is poor, and it is easy to overheat and soften during continuous cutting, and the cutting speed is less than 1000r.

[0003] After searching:

[0004] The document with Chinese patent application number CN201410809404.5 discloses "An Economical, Ultra-wide Saw Blade Steel and Its Manufacturing Method", whose components by weight percentage are: C: 0.35-0.45%, Si: 0.10-0.50%, Mn: 0.60-1.20%, P≤0.030%, S≤0.010%, B: 0.0010-0.0040%, Al: 0.010-0.080%, Ti≤0.060%, Ca: 0.0010-0.0080%, N≤0.0080%, O≤0.0080%, H≤0.0004%, and Nb0.001-0.050%, Cr0.01-0.50%, Mo0.01-0.50%, Ni0.01-0.50%, V One or more of 0.01-0.15%, and 0.15%≤(Cr / 5+Mn / 6+50B)≤0.45%, the rest is Fe and unavoidable impurities. The yield strength of the steel is greater than 850MPa, the tensile strength is 1000-1400MPa, the elongation is greater than 10%, and the Charpy V-type longitudinal impact energy can reach 50-90J. The present invention produces a steel plate with a thickness of 6.0-16.0mm through high-temperature final rolling, online water cooling, and tempering process, and then processes it into a saw blade body with a diameter of 1700-4500mm. The cross-sectional hardness of the entire saw blade body can reach 30-40HRC, and the hardness value is evenly distributed. Although the document improves the hardenability through manganese and boron, and adds a small amount of Nb, Cr, Mo, Ni, and V to optimize the performance, so that the hardness of the saw blade after quenching is 30-40HRC, this makes it impossible to meet the requirements of high-precision and high-speed cutting.

[0005] The document with Chinese patent application number CN201410333704.0 discloses "A high-carbon low-alloy saw blade steel and a method for producing hot-rolled steel plates thereof", the weight percentage of which chemical composition is C: 0.78-0.86%, Si: 0.15-0.40%, Mn: 0.40-0.70%, P≤0.025%, S≤0.015%, Al: 0.005-0.050%, Ca: 0-0.0050%, Cr: 0.50-0.80%, V: 0.15-0.25%, Ni≤0.25%, Cu≤0.20%, and the rest is Fe and unavoidable impurities; its hot-rolled steel plate manufacturing method includes blast furnace ironmaking, converter steelmaking, LF furnace refining, slab continuous casting, slab heating, hot rolling, hot rolled coil slow cooling and flattening and straightening steps. The steel produced according to the present invention has higher hardenability, hardenability and tempering resistance stability, has the characteristics of uniform structure and performance, good plate shape, low residual stress of steel plate, etc., and is suitable for manufacturing thick gauge and large size saw blades. The document optimizes the performance by Mn, Cr, and V. Although it can meet the high strength requirements, it cannot meet the high strength continuous working requirements because of the low Ni content. There is a risk of softening during use, and the cutting process needs to be cooled or the speed is reduced.

[0006] The document with Chinese patent application number CN201410655609.2 discloses a "high carbon low alloy saw blade steel for cutting stone and metal and a method for manufacturing the hot rolled steel plate thereof", wherein the mass percentage of chemical elements is: C: 0.70-0.80%; Si: 0.20-0.50%; Mn: 0.50-0.90%; P≤0.025%; S≤0.015%; Al: 0.005-0.050%; Cr: 0.30-0.60%; the rest is Fe and unavoidable impurities. The present invention also provides a method for manufacturing the hot rolled steel plate of high carbon low alloy saw blade steel for cutting stone and metal. By increasing the C, Cr and Mn content in the steel, the hardenability and hardenability of the steel are improved; by optimizing the process parameters of slab continuous casting, slab heating, hot rolling, coiling, slow cooling and straightening of hot rolled coils, the slab fracture and surface and internal cracks are avoided, and the problems of high strength, large residual stress and poor plate shape of the steel plate are solved. The composition of this document is similar to that of 75Cr1 saw blade steel, but due to its high Mn and Cr content, the saw blade is not only difficult to control the uniformity of stress distribution, but also has the same shortcomings of poor high temperature performance and easy softening.

[0007] The document with Chinese patent application number CN201510673626.3 discloses "A method for producing and smelting saw blade steel", and its process includes molten iron pretreatment → converter → LF refining → RH refining → slab continuous casting. Although this process is used to achieve stable control of the carbon content of saw blade steel, low sulfur, low hydrogen content and good continuous casting billet quality requirements: meet the requirements of the final finished product carbon content in the range of 0.30-0.60 weight %; low sulfur [S] ≤ 0.0030 weight %; low hydrogen content [H] ≤ 0.0002 weight %; various inclusion ratings ≤ 2.0; continuous casting billet center segregation level ≤ Class C 1.5, and realize the industrialized, batch and stable production of saw blade steel, but due to the low inclusion requirements in the document, fatigue fracture is prone to occur, and thus it cannot meet the requirements of high-speed cold cutting saw blades.

[0008] The document with Chinese patent application number CN201610122791.4 discloses "A hot-rolled coil for saw blade steel and its production method", whose chemical composition by weight percentage is C: 0.65-0.72%, Si: 0.15-0.30%, Mn: 1.10-1.30%, P: ≤0.025%, S: ≤0.020%, Als: 0.006-0.025%, Cr: 0.15-0.50%, and the balance is Fe and other inevitable impurities. The production method includes the following steps: converter smelting, LF refining, slab continuous casting, slab heating, controlled rolling, and coiling. The performance of the hot-rolled coil produced by the present invention after quenching and tempering treatment is tensile strength ≥800MPa, yield strength ≥500MPa, elongation ≥15%, and the structure is tempered troostite. The hot-rolled coil for saw blade steel meets the requirements of its subsequent heat treatment process for hardenability and plate shape. The composition of this document is similar to that of 65Mn-Cr saw blade steel. Due to its high manganese content, it is difficult to control the uniformity of stress distribution of the saw blade, and it cannot meet the sawing requirements of metal cold saw blades. Summary of the invention

[0009] The present invention aims to overcome the shortcomings of the prior art and provide a hot-rolled steel for a metal cold-cutting circular saw blade substrate and a production method thereof, which optimizes the hot-rolled plate production process, so that the cleanliness of the steel can reach inclusions ≤0.5 level, all of which are spherical D-type inclusions, the sum of PSN is less than 0.015%, the decarburized layer is controlled to 30-40 μm in the hot-rolled state, and the surface of the finished product has no decarburization characteristics, and at the same time, the metallographic structure is refined and uniform, the pearlite sheet spacing is 150-200 nm, so that the product produced by the prepared cold-cutting saw has accurate formability and significantly improved qualified rate.

[0010] Measures to achieve the above objectives:

[0011] A hot-rolled steel for a metal cold-cut circular saw blade substrate, the components and weight percentage contents of which are: C: 0.56-0.86%, Si: 0.10-0.50%, Mn: 0.20-1.00%, Cr: 0.20-1.00%, Ni: 0.40-1.50%, Mo: 0.01-0.30%, V: 0.01-0.30%, P≤0.010%, S≤0.003%, N≤0.002%, and the rest are Fe and inevitable impurities.

[0012] Preferably, the weight percentage of Cr is 0.65-0.95%.

[0013] Preferably, the weight percentage of Ni is 0.5-1.35%.

[0014] Preferably, the weight percentage content of Mo is 0.01-0.15%.

[0015] Preferably, the weight percentage of V is 0.01-0.12%.

[0016] A method for producing hot-rolled steel for a metal cold-cutting circular saw blade substrate, comprising the following steps:

[0017] 1) After converter smelting, LF refining is carried out, during which: the tapping temperature is controlled at 1600-1760°C, the tapping time is 4-15 minutes; the heating temperature of the molten steel in the LF furnace is controlled at 1500-1600°C;

[0018] 2) Perform RH vacuum treatment and control the vacuum degree at 30-50 Pa, cycle time 15-17 min, soft blowing 5-

[0019] 7min; calcium treatment Ca / S = 1.2-3.2, and make the inclusions spherical;

[0020] 3) After casting, heat the ingot, control the heating temperature of the ingot to be between 1300 and 1340°C, and the heating time to be between 120 and 180

[0021] min;

[0022] 4) Conventional rough rolling after high-pressure water descaling;

[0023] 5) Perform finish rolling, control the starting rolling temperature at 1100-1150°C, and the final rolling temperature at 820-920°C;

[0024] 6) Using front-stage cooling, cooling to 600-680°C at a cooling rate of 60-120°C / S;

[0025] 7) Coiling: Control the coiling temperature at 500-600°C;

[0026] 8) Reserved.

[0027] Functions and mechanisms of the components and main processes in the present invention

[0028] C: Carbon in steel mainly plays a role in improving the strength and hardenability of steel. In the hot-rolled structure, carbon exists in the form of carbides, forming pearlite, bainite, etc. After quenching, carbon exists in a solid solution state, and the structure undergoes phase transformation strengthening. After tempering, carbides precipitate, which plays a precipitation strengthening role. Too high carbon content will reduce the plasticity and toughness of steel, and too low carbon content will reduce the hardenability of steel, which is not conducive to the heat treatment of saw blade steel. The preferred range of carbon content in the present invention is controlled at 0.70-0.86%.

[0029] Si: Silicon in steel improves the strength of steel by solid solution strengthening and refining the pearlite plate spacing, but it reduces plasticity and toughness and increases surface defects of hot-rolled plates. Silicon is the main deoxidizer, and its content in steel is generally above 0.1%, so the preferred range of Si content is controlled at 0.16-0.38%.

[0030] Mn: Manganese in steel improves the strength of steel and combines with S in steel to form MnS, eliminating the effect of S. Mn is a good deoxidizer and can effectively refine pearlite, so the Mn content is preferably in the range of 0.36-0.60%.

[0031] Cr: Chromium can improve strength, hardenability and tempering resistance, and reduce the decarburization layer of hot-rolled plates. However, chromium will significantly increase the banded structure of steel and affect the uniformity of the structure. Therefore, the preferred range of Cr content is 0.36-0.66%.

[0032] Ni: Nickel can simultaneously improve the strength and toughness of steel, optimize welding performance and corrosion resistance, and improve low-temperature toughness. The preferred range of nickel content in the present invention is 0.50-1.00%.

[0033] V: Vanadium can refine the grain size, improve strength and toughness, and improve tempering resistance. The preferred range of V content in the present invention is 0.016-0.26%.

[0034] Mo: Molybdenum improves the strength of steel by solid solution strengthening and stabilizing carbides, and can also improve hardenability and inhibit temper brittleness. The preferred range of the content of the present invention is 0.016-0.26%.

[0035] P: Phosphorus comes from ores and is generally considered to be a harmful element in steel, which reduces the toughness and plasticity of steel. The lower the content in the present invention, the better, and the preferred range is 0.005%-0.010%.

[0036] S: Sulfur originates from coke, scrap steel, alloy and other steel smelting raw materials. It is generally considered to be a harmful element. It will increase the level of inclusions in steel, increase the level of segregation, reduce ductility and toughness, and cause hot working cracking. The lower the content of sulfur in the present invention, the better. The preferred range is 0.001%-0.003%.

[0037] N: Nitrogen originates from furnace gas and air in contact with molten steel during ironmaking and steelmaking. It has the effects of aging and grain refinement in steel, but has an adverse effect on toughness. The preferred range of nitrogen content in the present invention is 0.001%-0.002%.

[0038] The reason why the present invention controls the steel tapping temperature at 1600-1760°C and the steel tapping time at 4-15 minutes; the molten steel heating temperature in the LF furnace is controlled at 1500-1600°C is that high temperature is beneficial to reducing the phosphorus content in the steel, improving alloying and homogenization, and at the same time reducing the heating time of the next process and reducing the increase of nitrogen content.

[0039] The reason why the present invention controls the vacuum degree at 30-50Pa, the cycle time at 15-17min, the soft blowing at 5-7min, and the calcium treatment Ca / S at 1.2-3.2 is that low vacuum degree and long cycle time can accelerate the discharge of gas elements, and soft blowing and calcium treatment denature the inclusions in the steel and make them aggregate and float, thereby reducing the level of inclusions in the steel.

[0040] The reason why the present invention controls the heating temperature of the casting billet at 1300-1340°C is that high-temperature heating can homogenize the element segregation in the steel and improve the uniformity of the composition. At the same time, high temperature can effectively improve the dephosphorization efficiency and prevent the casting billet from being incompletely dephosphorized and causing the iron oxide scale to be pressed in.

[0041] The reason why the final rolling temperature is controlled at 820-920° C. in the present invention is that this temperature can ensure that the hot rolling is carried out in the austenite region and the grains are refined through austenite recrystallization.

[0042] The reason why the present invention controls cooling to 600-680°C at a cooling rate of 60-120°C / S is that rapid cooling can prevent high-temperature phase transformation, and controlling the phase transformation temperature at 600-680°C refines the pearlite plate spacing and homogenizes the structure.

[0043] The reason why the coiling temperature is controlled at 500-600°C in the present invention is that low-temperature phase transformation is beneficial to tissue refinement. When the temperature is lower than 500°C, martensite-bainite transformation is likely to occur to form a non-equilibrium tissue, increasing internal stress; when the temperature is higher than 600°C, segregation and banded tissue are likely to occur, forming tissue stress and affecting the stress uniformity of the finished product.

[0044] Compared with the prior art, the present invention optimizes the hot-rolled plate production process to improve the cleanliness of steel to achieve inclusions ≤0.5 level, all of which are spherical D-type inclusions, the sum of PSN <0.015%, the decarburization layer is controlled to 30-40um in the hot-rolled state, and the finished product surface has no decarburization characteristics. At the same time, the metallographic structure is refined and uniform, and the pearlite sheet spacing is 150-200nm, so that the product produced by the prepared cold cutting saw has accurate formability and significantly improved qualified rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a picture of the pearlite metallographic structure of the present invention. DETAILED DESCRIPTION

[0046] The present invention is described in detail below:

[0047] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;

[0048] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;

[0049] Table 3 is a table of performance test results of various embodiments and comparative examples of the present invention.

[0050] Each embodiment of the present invention is produced according to the following steps

[0051] 1) After converter smelting, LF refining is carried out, during which: the tapping temperature is controlled at 1600-1760°C, the tapping time is 4-15 minutes; the heating temperature of the molten steel in the LF furnace is controlled at 1500-1600°C;

[0052] 2) Perform RH vacuum treatment and control the vacuum degree at 30-50 Pa, cycle time 15-17 min, soft blowing 5-

[0053] 7min; calcium treatment Ca / S = 1.2-3.2, and make the inclusions spherical;

[0054] 3) After casting, heat the ingot, control the heating temperature of the ingot to be between 1300 and 1340°C, and the heating time to be between 120 and 180

[0055] min;

[0056] 4) Conventional rough rolling after high-pressure water descaling;

[0057] 5) Perform finish rolling, control the starting rolling temperature at 1100-1150°C, and the final rolling temperature at 820-920°C;

[0058] 6) Using front-stage cooling, cooling to 600-680°C at a cooling rate of 60-120°C / S;

[0059] 7) Coiling: Control the coiling temperature at 500-600°C;

[0060] 8) Reserved.

[0061] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)

[0062]

[0063]

[0064] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples

[0065]

[0066] Table 2

[0067]

[0068]

[0069] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples

[0070]

[0071] It can be seen from Table 3 that the hot-rolled product of the present invention has better plasticity than the comparative example, the inclusions and banded structure are also at a lower level, and the final stress distribution uniformity is better than the comparative example.

[0072] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.

Claims

1. A hot-rolled steel for a metal cold-cut circular saw blade substrate, wherein the components and weight percentage contents are: C: 0.56-0.86%, Si: 0.10-0.50%, Mn: 0.20-1.00%, Cr: 0.20-1.00%, Ni: 0.40-1.50%, Mo: 0.01-0.30%, V: 0.01-0.30%, P≤0.010%, S≤0.003%, N≤0.002%, and the rest is Fe and inevitable impurities.

2. The hot-rolled steel for a metal cold-cutting circular saw blade substrate as claimed in claim 1, characterized in that: The weight percentage of Cr is 0.65-0.95%.

3. The hot-rolled steel for a metal cold-cutting circular saw blade substrate as claimed in claim 1, characterized in that: The weight percentage content of Ni is 0.5-1.35%.

4. The hot-rolled steel for a metal cold-cutting circular saw blade substrate as claimed in claim 1, characterized in that: The weight percentage content of Mo is 0.01-0.15%.

5. The hot-rolled steel for a metal cold-cutting circular saw blade substrate as claimed in claim 1, characterized in that: The weight percentage of V is 0.01-0.12%.

6. A method for producing a hot-rolled steel for a metal cold-cutting circular saw blade substrate as claimed in claim 1, comprising the steps of: 1) After converter smelting, LF refining is carried out, during which: the tapping temperature is controlled at 1600-1760°C, the tapping time is 4-15 minutes; the heating temperature of the molten steel in the LF furnace is controlled at 1500-1600°C; 2) Perform RH vacuum treatment, and control the vacuum degree at 30-50Pa, the cycle time is 15-17min, and the soft blowing is 5-7min; calcium treatment Ca / S=1.2-3.2, and make the inclusions spherical; 3) After being cast into billets, the billets are heated, and the heating temperature of the billets is controlled at 1300-1340° C. and the heating time is 120-180 min; 4) Conventional rough rolling after high-pressure water descaling; 5) Perform finish rolling, control the starting rolling temperature at 1100-1150°C, and the final rolling temperature at 820-920°C; 6) Using front-stage cooling, cooling to 600-680°C at a cooling rate of 60-120°C / S; 7) Coiling: Control the coiling temperature at 500-600°C; 8) Reserved.

Citation Information

Patent Citations

  • Steel for saw blade substrate and manufacturing method thereof

    CN102134681A

  • High-carbon alloy steel, preparation method thereof and application of high-carbon alloy steel in saw blade tool

    CN116623081A

  • Fine pearlite corrosion-resistant hot-rolled saw blade steel and production method thereof

    CN118086765A

  • Economical saw blade matrix steel and production method thereof

    CN118086769A

  • Steel material for very low temperature use having excellent CTOD property after strain application, and method for manufacturing the same

    JP2013014812A

Cited By

  • Steel for saw blade and low-fracture-rate manufacturing method

    CN120738561A