Multi-component alloy air suction film system containing transition layer and preparation method of multi-component alloy air suction film system
By using a composite film system structure of a multi-component titanium alloy or zirconium alloy suction film and transition layer in MEMS devices, and using DC magnetron sputtering technology to deposit under vacuum conditions, the problem of poor bonding force between the getter film and the matrix is solved. Improves suction performance and adhesion, meeting the vacuum packaging needs of MEMS devices.
Patent Information
- Application Number
- CN202411073627.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The existing air-gass film has poor bonding power to the substrate, resulting in deflation pollution of the substrate and affecting the vacuum packaging performance of MEMS devices.
The composite film system of multi-component titanium alloy or zirconium alloy suction film and transition layer is used to deposit under vacuum through DC magnetron sputtering technology to form a dense transition layer and a suction film with uniformly distributed microcracks to improve the film Base bonding force and prevent the base from deflation.
It realizes high adhesion and high suction rate of the suction film system, improves the vacuum packaging performance of MEMS devices, avoids matrix pollution, and meets the vacuum packaging needs of microelectromechanical system devices.
Smart Images

Figure CN118979233A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of surface engineering, and in particular to a multi-element alloy gettering film system containing a transition layer and a preparation method thereof. Background Art
[0002] MEMS (micro-electromechanical systems) have made traditional vacuum sensors more miniaturized, with significant advantages such as small size, low power consumption, high sensitivity, good dynamic range and low production cost. Many MEMS devices, such as infrared detectors, accelerometers, gyroscopes, resonators, vibrating micro-mirrors, etc., must be operated in a vacuum environment to obtain satisfactory working performance. For example, an absolute pressure sensor must form a high vacuum cavity in its chip to provide an absolute reference pressure. The formation of a vacuum cavity is usually achieved through silicon-silicon bonding or silicon-glass bonding in a vacuum environment. After vacuum bonding packaging, maintaining the vacuum in the vacuum cavity is also an important issue.
[0003] Some transition metals and refractory metals, such as titanium, zirconium, hafnium, niobium, tungsten, tantalum, etc. and their alloys, have good adsorption properties for active gases at a certain temperature, and this property can be used to make getters. Getters are divided into two categories: evaporative and non-evaporative. Evaporative getters evaporate or sublimate the getter material to a surface to form a thin film getter (e.g., titanium sublimation pump). Evaporative getters require a high-temperature heat source, require a certain evaporation space, are difficult to control the evaporation direction, and are prone to pollution. They are difficult to use in current MEMS vacuum packaging and electric vacuum devices. Non-evaporable getters (NEG) do not require evaporation or sublimation. They only need to be activated at a certain temperature to work normally at room temperature. When traditional MEMS devices are vacuum packaged, getters are placed in a special space behind or adjacent to the MEMS chip chamber, and a channel connects the two spaces. Getters are generally porous structures sintered by powder metallurgy. During the placement of getters and the use of devices, small metal particles with a diameter of 2-3 microns will fall off from the getters. These small particles will have some significant impacts on the performance of the device: such as circuit short circuits, blocking of moving parts, causing resonant frequency drift, etc. The getter film is simpler, does not cause pollution, and increases the adsorption area. Using thin film deposition technology, the getter material is formed into a film in a silicon, glass or metal microchamber. Combined with the wafer bonding process, the vacuum packaging of MEMS devices can be carried out. The getter film is activated during the high-temperature bonding process to obtain and maintain the high vacuum of the reference cavity.
[0004] The getter membrane is generally a multi-component alloy of titanium or zirconium, with good getter performance and low activation temperature. However, the bonding strength between the membrane layer and certain substrates is poor. Although the substrate has been treated with chemical reagent cleaning, ion beam and bias cleaning, there is still a certain degree of contamination and outgassing on the surface. Therefore, effectively solving the poor bonding strength between the getter membrane and the substrate and preventing substrate outgassing pollution have become urgent problems to be solved. Summary of the invention
[0005] In view of the defects in the prior art, the purpose of the present invention is to provide a multi-element alloy gettering film system containing a transition layer and a preparation method thereof. A composite film system structure of a multi-element titanium alloy or zirconium alloy gettering film and a transition layer is adopted, and a DC magnetron sputtering technology is used to continuously prepare film layers without destroying the vacuum, so as to achieve high adhesion and high gettering rate of the gettering film system and improve the comprehensive performance of the gettering film system.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] In the first aspect, the present invention provides a multi-element alloy gettering film system containing a transition layer, comprising: a transition layer and a multi-element alloy gettering film layer, wherein the transition layer is deposited on the surface of a substrate, and the multi-element alloy gettering film layer is deposited on the surface of the transition layer; the transition layer is a dense structure film with a thickness of 10 to 100 nm; the multi-element alloy gettering film layer is a cluster structure film with a large number of microcracks evenly distributed, with a thickness of 1 to 5 μm; the material of the transition layer is Ti or Cr, and the material of the multi-element alloy gettering film layer is a Ti alloy or a Zr alloy.
[0008] Furthermore, the Ti alloy comprises, by mass percentage, 50% to 85% Ti, 10% to 40% auxiliary gettering elements, and 1% to 10% doping elements, wherein the auxiliary gettering elements include one of Co, V, Mn, and Al, and the doping elements include one or more of Fe, Hf, Nb, Y, La, Ce, Pr, and Nd.
[0009] Furthermore, the Zr alloy comprises, by mass percentage, 50% to 85% Zr, 10% to 40% auxiliary gettering elements, and 1% to 10% doping elements, wherein the auxiliary gettering elements comprise one of Co, V, Mn, and Al, and the doping elements comprise one or more of Fe, Hf, Nb, Y, La, Ce, Pr, and Nd.
[0010] Furthermore, the substrate is a rigid or flexible substrate, and the material of the substrate is silicon, metal, ceramic or glass.
[0011] In a second aspect, the present invention provides a method for preparing a multi-element alloy getter film system containing a transition layer, comprising the following steps:
[0012] Step (1) The substrate surface is cleaned with chemical reagents or ultrasonic cleaning, and then blown dry with pure dry nitrogen in a clean bench for later use;
[0013] Step (2) placing the substrate on a workbench in a vacuum chamber, adjusting the workbench so that the distance between the surface of the substrate and the surface of the sputtering target is 5 to 15 cm, and evacuating the vacuum chamber to a vacuum level of ≤1×10 -2 Pa, 150~200℃ heating and baking to degas;
[0014] Step (3) After the vacuum is evacuated to the background vacuum, a high-purity inert gas is introduced into the vacuum chamber, a bias power supply is turned on, and an ion source is turned on at the same time to perform ion beam activation and bias cleaning on the surface of the substrate;
[0015] Step (4) adjusting the inert gas flow rate to the gas pressure required for transition layer deposition, using DC magnetron sputtering, turning on the transition layer target power supply, and pre-sputtering for 5 to 15 minutes before depositing the transition layer;
[0016] Step (5) rotates the workbench to below the getter film target, adjusts the inert gas flow rate to the gas pressure required for getter film deposition, uses DC magnetron sputtering, turns on the getter film sputtering target power supply, and performs getter film deposition after pre-sputtering for 5 to 15 minutes.
[0017] Furthermore, in step (3), the background vacuum is ≤10 -4 Pa, after the inert gas is introduced, the gas pressure is maintained at 0.1~3.0Pa, the applied bias voltage is 100V~500V, the ion source working voltage is 1.0kV~5.0kV, and the action time is 10min~30min.
[0018] Furthermore, in step (4), the inert gas flow rate is adjusted to a gas pressure of 0.1 to 1.0 Pa required for transition layer deposition, the DC sputtering power is 100 W to 500 W, the transition layer deposition time is 3 to 10 min, and the workbench rotation speed is 5 to 20 r / min.
[0019] Furthermore, in step (5), the inert gas flow rate is adjusted to a gas pressure of 2.0 to 10.0 Pa required for the deposition of the absorbent film layer, the DC sputtering power is 200 W to 500 W, the absorbent film layer deposition time is 20 to 60 min, and the workbench rotation speed is 5 to 20 r / min.
[0020] The technical solution of the present invention has the following advantages:
[0021] The air-intake film system provided by the present invention is a composite double-layer film system structure of a multi-component titanium alloy or zirconium alloy air-intake film and a transition layer. The transition layer is first deposited on the surface of the substrate, and then the alloy air-intake film is deposited on the surface of the transition layer. On the one hand, the bonding force between the air-intake film system and the substrate is improved, and on the other hand, the contamination of the substrate outgassing is avoided, thereby improving the air-intake performance. The present invention adopts DC magnetron sputtering technology to continuously prepare film layers without breaking the vacuum. During the preparation process, the microscopic morphology of the film is regulated by adjusting the process parameters, thereby further improving the air-intake performance of the film. The multi-component alloy air-intake film system containing a transition layer of the present invention has high adhesion and high air-intake rate, and has excellent comprehensive performance, meeting the vacuum packaging requirements of micro-electromechanical system devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a schematic structural diagram of a multi-element alloy gettering film system including a transition layer provided in an embodiment of the present application;
[0023] Figure 2 2(a) is a surface and cross-sectional micrograph of a multi-element alloy gettering film system containing a transition layer prepared according to Example 1 of the present application, wherein 2(a) is a surface morphology of the multi-element alloy gettering film layer, and 2(b) is a cross-sectional morphology of the multi-element alloy gettering film system containing a transition layer;
[0024] Figure 3 is a gettering performance curve of a multi-element alloy gettering film system containing a transition layer prepared according to an embodiment of the present application;
[0025] In the figure, 1-substrate, 2-transition layer, 3-multi-alloy gettering film layer. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.
[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so as to describe the embodiments of the present application described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0028] In the present application, the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inner", "outer", "middle", "vertical", "horizontal", "lateral", "longitudinal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings. These terms are mainly used to better describe the present application and its embodiments, and are not used to limit the indicated devices, elements or components to have a specific orientation, or to be constructed and operated in a specific orientation.
[0029] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those of ordinary skill in the art, the specific meanings of these terms in this application can be understood according to specific circumstances.
[0030] In addition, the term "plurality" shall mean two or more.
[0031] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0032] The technical problem to be solved by the present invention is to overcome the problems of poor bonding between the getter film and the substrate and outgassing pollution of the substrate in the prior art. To this end, the present invention provides a multi-element alloy getter film system containing a transition layer and a preparation method thereof.
[0033] See also Figure 1 The structure of the multi-element alloy gettering film system containing a transition layer provided in an embodiment of the present invention is as follows: Figure 1As shown. First, a transition layer 2 is deposited on the surface of the substrate 1, and then a multi-element alloy gettering layer 3 is deposited on the surface of the transition layer 2 to form a double-layer structure gettering film system. On the one hand, the film-base bonding strength is improved, and on the other hand, the contamination of the substrate outgassing is avoided, thereby improving the gettering performance. The substrate 1 is a rigid or flexible substrate of silicon, metal, ceramic or glass material. The composition of the transition layer 2 is Cr or Ti, and the thickness is 10 to 100nm; the composition of the multi-element alloy gettering film layer 3 is Ti alloy or Zr alloy, and the thickness is 1 to 5μm.
[0034] See also Figure 2 2(a) is the surface morphology of the multi-element alloy gettering film layer, and 2(b) is the cross-sectional morphology of the multi-element alloy gettering film system containing a transition layer. Figure 2 As shown, the transition layer 2 has a dense structure, and the multi-element alloy gettering film layer 3 has a cluster structure with a large number of microcracks evenly distributed.
[0035] Furthermore, in terms of mass percentage, the composition of the Ti alloy includes: 50% to 85% Ti, 10% to 40% auxiliary gettering elements, and 1% to 10% doping elements; the composition of the Zr alloy includes: 50% to 85% Zr, 10% to 40% auxiliary gettering elements, and 1% to 10% doping elements.
[0036] Specifically, the auxiliary gettering element includes one of Co, V, Mn, and Al, and the doping element includes one or more of Fe, Hf, Nb, Y, La, Ce, Pr, and Nd.
[0037] Furthermore, DC magnetron sputtering technology is used to continuously prepare a multi-element alloy gettering film system containing a transition layer without breaking the vacuum. During the preparation process, the microscopic morphology of the film is controlled by adjusting the process parameters. First, a transition layer 2 is formed on the surface of the substrate 1 by DC magnetron sputtering deposition, and a multi-element alloy gettering film layer 3 is formed on the surface of the transition layer 2 by DC magnetron sputtering deposition, forming a double-layer gettering film system structure, which effectively improves the film-base bonding force, while avoiding the influence of outgassing and impurities on the surface of the substrate, thereby improving the adhesion and gettering performance, and meeting the vacuum packaging requirements of MEMS devices.
[0038] See also Figure 3 At 350°C, the multi-element alloy gas absorption film system containing a transition layer prepared in the embodiment was activated, and the hydrogen absorption performance test was carried out after 15 minutes. The hydrogen absorption performance curve is as follows: Figure 3 shown.
[0039] Example 1
[0040] This embodiment provides a multi-element alloy gettering film system containing a transition layer, comprising: a quartz glass substrate, a Cr transition layer deposited on the surface of the quartz glass, and a Zr alloy gettering film layer deposited on the surface of the Cr transition layer. In terms of mass percentage, the composition of the Zr alloy gettering film layer is Zr81%-Co14%-La5%. The thickness of the Cr transition layer is 20nm, and the thickness of the Zr alloy gettering film layer is 2μm.
[0041] The method for preparing the multi-element alloy getter film system containing a transition layer in this embodiment comprises the following steps:
[0042] Step (1) Take an area of 1 to 16 cm 2 The quartz glass sheet was used as the substrate, which was ultrasonically cleaned with acetone, alcohol and deionized water, and then dried with pure nitrogen on a clean bench for later use.
[0043] Step (2) Place a quartz glass sheet on a workbench in a vacuum chamber, adjust the workbench so that the distance between the surface of the quartz glass sheet and the surface of the sputtering target is 6 cm, and evacuate to 10 -3 Pa, 150℃ heating and baking for degassing;
[0044] Step (3) Pump down to background vacuum ≤ 10 -4 After 1 Pa, high-purity krypton gas (purity ≥ 99.99%) was introduced into the vacuum chamber to keep the gas pressure at 1 Pa, the bias power supply was turned on, a bias voltage of 500 V was applied, and the ion source was turned on at the same time, the ion source voltage was 2 kV, and the surface of the quartz glass sheet was ion beam activated and bias cleaned for 10 min;
[0045] Step (4) adjusting the krypton gas flow rate to the gas pressure (0.3 Pa) required for transition layer deposition, performing DC magnetron sputtering, the transition layer sputtering target is high-purity Cr (purity ≥ 99.95%), turning on the transition layer sputtering target power supply, the sputtering power is 200 W, and the transition layer deposition is started after pre-sputtering for 5 minutes, the deposition time is 5 minutes, and the workbench rotation speed is 10 r / min;
[0046] Step (5) rotate the workbench to below the getter film target, adjust the krypton gas flow rate to the gas pressure (4.0 Pa) required for getter film deposition, perform DC magnetron sputtering, the getter film sputtering target is Zr81%-Co14%-La5% (purity ≥99.5%), turn on the getter film sputtering target power supply, the sputtering power is 300 W, start getter film deposition after pre-sputtering for 5 minutes, the deposition time is 30 minutes, and the workbench rotation speed is 10 r / min.
[0047] The morphology of the multi-element alloy getter film system containing a transition layer prepared in this embodiment was observed by scanning electron microscopy. The cross-sectional morphology is as follows: Figure 2 (b) shows the surface morphology of the multi-element alloy gettering film layer. Figure 2 (a) shown.
[0048] At 350°C, the multi-element alloy gas absorption film system containing a transition layer prepared in this embodiment was activated, and the hydrogen absorption performance test was performed after 15 minutes. The hydrogen absorption performance curve is shown in Figure 3 Curve 1 in .
[0049] Example 2
[0050] This embodiment provides a multi-element alloy gettering film system containing a transition layer, comprising: a single crystal silicon wafer substrate, a Cr transition layer deposited on the surface of the single crystal silicon wafer, and a Zr alloy gettering film layer deposited on the surface of the Cr transition layer. In terms of mass percentage, the composition of the Zr alloy gettering film layer is Zr70%-V24.6%-Fe5.4%. The thickness of the Cr transition layer is 50nm, and the thickness of the Zr alloy gettering film layer is 2.2μm.
[0051] The method for preparing the multi-element alloy getter film system containing a transition layer in this embodiment comprises the following steps:
[0052] Step (1) A single crystal silicon wafer with a diameter of ≤10 cm is taken as a substrate, and ultrasonically cleaned with acetone, alcohol and deionized water in sequence, and then blown dry with pure nitrogen on a clean bench for later use;
[0053] Step (2) Place the single crystal silicon wafer on a workbench in the vacuum chamber, adjust the workbench so that the distance between the surface of the single crystal silicon wafer and the surface of the sputtering target is 7 cm, and evacuate to 10 -3 Pa, 150℃ heating and baking for degassing;
[0054] Step (3) Pump down to background vacuum ≤ 10 -4 After 1 Pa, high-purity krypton gas (purity ≥ 99.99%) is introduced into the vacuum chamber to keep the gas pressure at 1 Pa. The bias power supply is turned on and a bias voltage of 500 V is applied. At the same time, the ion source is turned on and the ion source voltage is 2 kV. The surface of the single crystal silicon wafer is ion beam activated and bias cleaned for 10 minutes:
[0055] Step (4) adjusting the krypton gas flow rate to the gas pressure (0.3 Pa) required for transition layer deposition, performing DC magnetron sputtering, the transition layer sputtering target is high-purity Cr (purity ≥ 99.95%), turning on the transition layer sputtering target power supply, the sputtering power is 300 W, and the transition layer deposition is started after pre-sputtering for 5 minutes, the deposition time is 5 minutes, and the workbench rotation speed is 10 r / min;
[0056] Step (5) rotate the workbench to below the getter film target, adjust the krypton gas flow rate to the gas pressure (3.0 Pa) required for getter film deposition, perform DC magnetron sputtering, the getter film sputtering target is Zr70%-V24.6%-Fe5.4% (purity ≥99.5%), turn on the getter film sputtering target power supply, the sputtering power is 350 W, start getter film deposition after pre-sputtering for 5 minutes, the deposition time is 20 minutes, and the workbench rotation speed is 10 r / min.
[0057] At 350°C, the multi-element alloy gas absorption film system containing a transition layer prepared in this embodiment was activated, and the hydrogen absorption performance test was carried out after 15 minutes. The hydrogen absorption performance curve is shown in FIG. Figure 3 Curve 2 in .
[0058] Example 3
[0059] This embodiment provides a multi-element alloy gettering film system containing a transition layer, comprising: a stainless steel thin disc substrate, a Ti transition layer deposited on the surface of the stainless steel thin disc, and a Ti alloy gettering film layer deposited on the surface of the Ti transition layer. In terms of mass percentage, the composition of the Ti alloy gettering film layer is Ti70%-V25%-Hf5%. The thickness of the Ti transition layer is 30nm, and the thickness of the Ti alloy gettering film layer is 2.4μm.
[0060] The method for preparing the multi-element alloy getter film system containing a transition layer in this embodiment comprises the following steps:
[0061] Step (1) A stainless steel thin disc with a thickness of 150 μm and a diameter of ≤10 cm is used as a substrate, and ultrasonically cleaned with acetone, alcohol and deionized water in succession, and then blown dry with pure nitrogen on a clean bench for later use;
[0062] Step (2) Place a stainless steel thin disc on a workbench in a vacuum chamber, adjust the workbench so that the distance between the surface of the stainless steel thin disc and the surface of the sputtering target is 6 cm, and evacuate to 10 -3 Pa, 150℃ heating and baking for degassing;
[0063] Step (3) Pump down to background vacuum ≤ 10 -4 After 1 Pa, high-purity krypton gas (purity ≥ 99.99%) was introduced into the vacuum chamber to keep the gas pressure at 1 Pa, the bias power supply was turned on, a bias voltage of 500 V was applied, and the ion source was turned on at the same time, the ion source voltage was 2 kV, and the surface of the stainless steel thin disc was ion beam activated and bias cleaned for 10 min;
[0064] Step (4) adjusting the krypton gas flow rate to the gas pressure (0.2 Pa) required for transition layer deposition, performing DC magnetron sputtering, the transition layer sputtering target is high-purity Ti (purity ≥ 99.995%), turning on the transition layer sputtering target power supply, the sputtering power is 200 W, and the transition layer deposition is started after pre-sputtering for 5 minutes, the deposition time is 5 minutes, and the workbench rotation speed is 10 r / min;
[0065] Step (5) rotate the workbench to below the getter film target, adjust the krypton gas flow rate to the gas pressure (3.0 Pa) required for getter film deposition, perform DC magnetron sputtering, the getter film sputtering target is Ti70%-V25%-Hf5% (purity ≥99.5%), turn on the getter film sputtering target power supply, the sputtering power is 300 W, start getter film deposition after pre-sputtering for 5 minutes, the deposition time is 30 minutes, and the workbench rotation speed is 10 r / min.
[0066] At 350°C, the multi-element alloy gas absorption film system containing a transition layer prepared in this embodiment was activated, and the hydrogen absorption performance test was carried out after 15 minutes. The hydrogen absorption performance curve is shown in FIG. Figure 3 Curve 3 in .
[0067] Example 4
[0068] This embodiment provides a multi-element alloy gettering film system containing a transition layer, comprising: a single crystal silicon wafer substrate, a Cr transition layer deposited on the surface of the single crystal silicon wafer, and a Zr alloy gettering film layer deposited on the surface of the Cr transition layer. In terms of mass percentage, the composition of the Zr alloy gettering film layer is Zr81%-Co14%-La5%. The thickness of the Cr transition layer is 30nm, and the thickness of the Zr alloy gettering film layer is 2.8μm.
[0069] The method for preparing the multi-element alloy getter film system containing a transition layer in this embodiment comprises the following steps:
[0070] Step (1) A single crystal silicon wafer with a diameter of ≤10 cm is taken as a substrate, and ultrasonically cleaned with acetone, alcohol and deionized water in sequence, and then blown dry with pure nitrogen on a clean bench for later use;
[0071] Step (2) Place a single crystal silicon wafer on a workbench in a vacuum chamber, adjust the workbench so that the distance between the surface of the single crystal silicon wafer and the surface of the sputtering target is 6 cm, and evacuate to 10 -3 Pa, 150℃ heating and baking for degassing;
[0072] Step (3) Pump down to background vacuum ≤ 10 -4After 2 Pa, high-purity argon gas (purity ≥ 99.99%) was introduced into the vacuum chamber to keep the gas pressure at 2 Pa, the bias power supply was turned on, a bias voltage of 500 V was applied, and the ion source was turned on at the same time, the ion source voltage was 2 kV, and the surface of the single crystal silicon wafer was ion beam activated and bias cleaned for 10 minutes;
[0073] Step (4) adjusting the argon flow rate to the gas pressure (0.5 Pa) required for transition layer deposition, performing DC magnetron sputtering, the transition layer sputtering target is high-purity Cr (purity ≥ 99.95%), turning on the transition layer sputtering target power supply, the sputtering power is 200 W, and the transition layer deposition is started after pre-sputtering for 5 minutes, the deposition time is 5 minutes, and the workbench rotation speed is 10 r / min;
[0074] Step (5) rotate the workbench to the bottom of the getter film target, adjust the argon flow rate to the gas pressure (6.0Pa) required for getter film deposition, and perform DC magnetron sputtering. The getter film sputtering target is Zr81%-C014%-La5% (purity ≥99.5%). Turn on the getter film sputtering target power supply, the sputtering power is 400W, and start getter film deposition after pre-sputtering for 10 minutes. The deposition time is 40 minutes, and the workbench rotation speed is 10r / min.
[0075] At 350°C, the multi-element alloy gas absorption film system containing a transition layer prepared in this embodiment was activated, and the hydrogen absorption performance test was performed after 15 minutes. The hydrogen absorption performance curve is shown in Figure 3 Curve 4 in .
[0076] Experimental example
[0077] The morphology of the multi-element alloy getter film system containing a transition layer prepared in Example 1 was observed by scanning electron microscopy. The cross-sectional morphology is as follows: Figure 2 (b) shows the surface morphology of the multi-element alloy gettering film layer. Figure 2 (a) shown.
[0078] Figure 2 As shown, a Cr transition layer with a thickness of 20 nm is first deposited on the surface of the quartz glass substrate, and then a Zr81%-Co14%-La5% alloy gettering film layer with a thickness of 2 μm is deposited on the surface of the Cr transition layer to form a double-layer gettering film system. The transition layer has a dense structure, and the alloy gettering film layer has a cluster structure with a large number of uniformly distributed microcracks.
[0079] The hydrogen absorption performance of the multi-element alloy absorption film system containing the transition layer prepared in Examples 1 to 4 of the present invention was tested, and the hydrogen absorption performance curve is shown in FIG. Figure 3 The preparation processes and membrane hydrogen absorption performance test results of Examples 1 to 4 of the present invention are shown in Table 1.
[0080] Table 1 Preparation process of Examples 1 to 4 and test results of membrane system hydrogen absorption performance
[0081]
[0082] As shown in Table 1, Example 1 uses a Zr81%-Co14%-La5% alloy gettering film, the thickness of the Cr transition layer is 20nm, the thickness of the Zr alloy gettering film layer is 2μm, krypton gas is used for magnetron sputtering, and the sputtering pressure is 4.0Pa: Example 2 uses a Zr70%-V24.6%-Fe5.4% alloy gettering film, the thickness of the Cr transition layer is 50nm, the thickness of the Zr alloy gettering film layer is 2.2μm, krypton gas is used for magnetron sputtering, and the sputtering pressure is 3. 0Pa; Example 3 uses Ti70%-V25%-Hf5% alloy gettering film, the thickness of the Ti transition layer is 30nm, the thickness of the Ti alloy gettering film layer is 2.4μm, krypton gas is used for magnetron sputtering, and the sputtering pressure is 3.0Pa: Example 4 uses Zr81%-Co14%-La5% alloy gettering film, the thickness of the Cr transition layer is 30nm, the thickness of the Zr alloy gettering film layer is 2.8μm, argon gas is used for magnetron sputtering, and the sputtering pressure is 6.0Pa. At 350℃, the multi-element alloy gettering film system containing the transition layer prepared in Examples 1 to 4 was activated, and the hydrogen absorption performance was tested after 15 minutes. Figure 3 As shown in the figure, the initial hydrogen absorption rates of the multi-element alloy absorption films containing transition layers prepared in Examples 1 to 4 are 205 ml / S / cm 2 、178ml / S / cm 2 、132ml / S / cm 2 、100ml / S / cm 2 , the hydrogen absorption performance curves correspond to Figure 3 Curves 1, 2, 3 and 4. It can be seen that the hydrogen absorption performance of the multi-element alloy gettering film system containing a transition layer prepared in the embodiment of the present invention is improved, and the krypton sputtering process can better improve the gettering performance by using the same alloy gettering film composition.
[0083] To sum up, the multi-alloy gettering film system containing a transition layer prepared in the embodiment of the present invention is a double-layer gettering film system structure, which is continuously prepared by DC magnetron sputtering technology without breaking the vacuum. During the preparation process, the microscopic morphology of the film is regulated by adjusting the process parameters, thereby effectively improving the bonding strength of the film and the substrate, while avoiding the influence of outgassing and impurities on the surface of the substrate, thereby improving the adhesion and gettering performance, and meeting the vacuum packaging requirements of micro-electromechanical system devices.
[0084] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A multi-element alloy getter film system containing a transition layer, characterized in that: include: A transition layer and a multi-element alloy gettering film layer, wherein the transition layer is deposited on the surface of a substrate, and the multi-element alloy gettering film layer is deposited on the surface of the transition layer; the transition layer is a dense structure film with a thickness of 10 to 100 nm; the multi-element alloy gettering film layer is a cluster structure film with a large number of microcracks evenly distributed, with a thickness of 1 to 5 μm; the material of the transition layer is Ti or Cr, and the material of the multi-element alloy gettering film layer is a Ti alloy or a Zr alloy.
2. The multi-element alloy gettering film system containing a transition layer according to claim 1, characterized in that: Calculated by mass percentage, the Ti alloy includes: 50% to 85% Ti, 10% to 40% auxiliary gettering elements, and 1% to 10% doping elements; calculated by mass percentage, the Zr alloy includes: 50% to 85% Zr, 10% to 40% auxiliary gettering elements, and 1% to 10% doping elements, wherein the auxiliary gettering element includes one of Co, V, Mn, and Al, and the doping element includes one or more of Fe, Hf, Nb, Y, La, Ce, Pr, and Nd.
3. The multi-element alloy gettering film system containing a transition layer according to claim 1, characterized in that: The substrate is a rigid or flexible substrate, and the material of the substrate is silicon, metal, ceramic or glass.
4. The method for preparing a multi-element alloy gettering film system containing a transition layer according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step (1) The substrate surface is cleaned with chemical reagents or ultrasonic cleaning, and then blown dry with pure dry nitrogen in a clean bench for later use; Step (2) placing the substrate on a workbench in a vacuum chamber, adjusting the workbench so that the distance between the surface of the substrate and the surface of the sputtering target is 5 to 15 cm, and evacuating the vacuum chamber to a vacuum level of ≤1×10 -2 pa, 150~200℃ heating and baking to degas; Step (3) After the vacuum is evacuated to the background vacuum, a high-purity inert gas is introduced into the vacuum chamber, a bias power supply is turned on, and an ion source is turned on at the same time to perform ion beam activation and bias cleaning on the surface of the substrate; Step (4) adjusting the inert gas flow rate to the gas pressure required for transition layer deposition, using DC magnetron sputtering, turning on the transition layer target power supply, and pre-sputtering for 5 to 15 minutes before depositing the transition layer; Step (5) rotates the workbench to below the getter film target, adjusts the inert gas flow rate to the gas pressure required for getter film deposition, uses DC magnetron sputtering, turns on the getter film sputtering target power supply, and performs getter film deposition after pre-sputtering for 5 to 15 minutes.
5. The method for preparing a multi-component alloy gettering film system containing a transition layer according to claim 4, characterized in that: In the step (3), the background vacuum is ≤10 -4 Pa, after the inert gas is introduced, the gas pressure is maintained at 0.1~3.0Pa, the applied bias voltage is 100V~500V, the ion source working voltage is 1.0kV~5.0kV, and the action time is 10min~30min.
6. The method for preparing a multi-component alloy gettering film system containing a transition layer according to claim 4, characterized in that: In the step (4), the inert gas flow rate is adjusted to a gas pressure of 0.1 to 1.0 Pa required for transition layer deposition, the DC sputtering power is 100 W to 500 W, the transition layer deposition time is 3 to 10 min, and the workbench rotation speed is 5 to 20 r / min.
7. The method for preparing a multi-element alloy gettering film system containing a transition layer according to claim 4, characterized in that: In the step (5), the inert gas flow rate is adjusted to a gas pressure of 2.0 to 10.0 Pa required for the deposition of the absorbent film layer, the DC sputtering power is 200 W to 500 W, the absorbent film deposition time is 20 to 60 min, and the workbench rotation speed is 5 to 20 r / min.
Citation Information
Cited By
Ion accelerator electron cooling vacuum system and vacuum obtaining method thereof
CN122513916A