Method for converting zinc coating into ZIF-8 thin film in situ and SPME probe based on ZIF-8 thin film
By electrochemically preparing the galvanized layer and converting it into ZIF-8 film at room temperature and normal pressure, it solves the problems of ZIF-8 coating thickness control and mass production, improves the mechanical strength and extraction efficiency of the SPME probe, and reduces costs and equipment Demand, suitable for trace analysis.
Patent Information
- Application Number
- CN202410928816.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-19
AI Technical Summary
When using ZIF-8 as the SPME probe coating material in the prior art, the coating thickness is not easy to be accurately controlled, the sol blocks the pores of ZIFs, is difficult to batch production, requires a large amount of organic solvent, and requires heating/pressurization, which limits its application range.
The galvanized layer was prepared on a metal carrier by electrochemical method, and the galvanized layer was converted into a ZIF-8 film in situ under normal pressure conditions in room temperature, avoiding pore blockage and high temperature and high pressure requirements during sol fixation, and achieving thickness and precise control of density reduces reagent consumption and equipment requirements.
It realizes accurate thickness control of ZIF-8 film, improves mechanical strength and extraction efficiency, reduces production costs and equipment requirements, and is suitable for batch preparation and trace analysis.
Smart Images

Figure CN118979247A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solid phase microextraction, in particular to a method for in-situ converting a zinc coating into a ZIF-8 film and an SPME probe based on the ZIF-8 film. Background Art
[0002] Solid Phase Microextraction (SPME) is a green sample pretreatment technology that can concentrate and sample the substances to be tested in the sample without using organic solvents or using a small amount of organic solvents. When used in conjunction with instruments such as GC, HPLC, and MS, it can achieve rapid quantitative analysis of trace organic matter in the sample. Therefore, SPME has become a simple method that can replace liquid-liquid extraction.
[0003] SPME probes have been commercialized by Supelco in the United States, and their coatings mainly include PDMS (polydimethylsiloxane), PA (polyacrylate), CAR / PDMS (polyethylene glycol / polydimethylsiloxane), CW / DVB (carbon molecular sieve / vinylbenzene) and CW / TPR (carbon molecular sieve / molecular template resin). The preparation method of these coatings is to fix the polymer on the surface of the carrier by light or heating, and the early commercialized probes are mainly based on fused quartz fibers as carriers, which have low mechanical strength and are very easy to break during use. Although there are commercial SPME probes with carriers such as nickel-titanium alloy wires, these commercial probes are expensive, the recommended operating temperature is low, and the coating will swell when measuring samples containing organic solvents. These defects greatly limit the scope of use of SPME technology.
[0004] The SPME probe consists of a carrier (such as quartz fiber, nickel-titanium alloy wire, stainless steel wire, etc.) that carries the coating and an adsorbed coating on the carrier. It is the core of the SPME technology. At present, the development of SPME probes mainly focuses on the following aspects: first, solving the mechanical strength of the carrier and improving its service life; second, selecting a suitable adsorbent to improve the enrichment efficiency and solve its ability to resist organic solvents; third, developing a production method that can minimize costs; fourth, it can be prepared in batches under mild conditions. In terms of the mechanical strength of the probe, predecessors have used stainless steel wire, copper wire, aluminum wire, nickel-titanium alloy wire and other metal (metal alloy) wires with high mechanical strength as carriers to solve the problem of the mechanical strength of the probe; and in terms of selecting new materials with high extraction efficiency, analytical chemists have also done a lot of work, such as using activated carbon, carbon nanotubes, polyionic liquids, metal organic framework materials, covalent organic framework materials, etc. as coating materials have also been successful, especially metal organic framework materials as adsorption coating materials have also been studied a lot. Metal Organic Frameworks (MOFs) materials are organic-inorganic hybrid materials with intramolecular pores formed by the assembly of organic ligands (such as imidazole, organic carboxylic acid, etc.) and metal ions (such as zinc, copper, iron, aluminum, cobalt, nickel, etc.) through coordination bonds. MOFs are ideal adsorption materials for SPME coatings because of their huge specific surface area, customizable pore structure, and extremely high chemical / thermal stability.
[0005] Zeolitic Imidazolate Frameworks (ZIFs) are a subclass of MOFs. They are a new type of MOFs with a zeolite topological structure formed by divalent transition metal ions and imidazole ligands. ZIFs not only have the advantages of MOFs materials such as adjustable pore size and large surface area, but also have greatly improved thermal stability, chemical stability and water stability compared to other MOFs materials. They have been widely used in gas separation, adsorption, storage and catalysis. Among the many ZIFs materials, ZIF-8 is the most studied and widely used. ZIF-8 is usually prepared by solvothermal method of 2-methylimidazole ligand and zinc salt (zinc nitrate, zinc acetate, etc.), which generally requires high temperature, high pressure, and long reaction time, and also requires a large amount of organic solvent (such as methanol, DMF, etc.).
[0006] In the reports on using ZIF-8 as a coating material to make SPME probes, the main methods are as follows: 1. First synthesize ZIF-8, and then fix it on the carrier by sol-gel method, adhesive method, etc.; 2. Introduce a seed layer on the carrier, and then perform hydrothermal / solvothermal in situ growth; 3. Physical adhesion; 4. Electrochemical preparation. However, these preparation methods have different degrees of shortcomings such as the coating thickness is not easy to accurately control, the sol blocks the pores of ZIFs, requires a large amount of organic solvents, is difficult to batch produce, and requires heating / pressurization. Summary of the invention
[0007] The present invention aims to provide a method for in-situ conversion of a zinc coating into a ZIF-8 film and an SPME probe based on the ZIF-8 film, so as to solve the technical problems that when ZIF-8 is used as a coating material to make an SPME probe, the coating thickness is not easy to accurately control, the sol blocks the pores of ZIFs, it is difficult to make in batches, a large amount of organic solvent is required, and heating / pressurization is required.
[0008] In order to achieve the above-mentioned purpose, the specific scheme adopted by the present invention is: a method for in-situ conversion of a zinc-plated layer into a ZIF-8 film, comprising the following steps: S1: preparing a zinc-plated layer on a metal carrier; S2: mixing 2-methylimidazole, sodium formate, methanol and ammonia water to obtain a conversion liquid; S3: immersing the metal carrier with a zinc-plated layer in step S1 in the conversion liquid obtained in step S2, allowing the reaction to stand at room temperature, and converting the zinc-plated layer into a ZIF-8 film in situ.
[0009] As a further optimization of the above technical solution, step S1 is specifically: using a conductive metal carrier as a working electrode, a saturated calomel electrode as a reference electrode, a platinum wire as a counter electrode, and an aqueous zinc sulfate solution as an electrolyte, controlling the voltage and time, and electroplating zinc on the metal carrier to obtain a zinc-plated layer.
[0010] As a further optimization of the above technical solution, the metal carrier is stainless steel wire, aluminum wire, copper wire, nickel-titanium alloy wire, metal plate or blank SPME arrow.
[0011] As a further optimization of the above technical solution, before step S1, the metal carrier is ultrasonically cleaned with ethanol and deionized water respectively.
[0012] As a further optimization of the above technical solution, in step S2, the molar ratio of 2-methylimidazole to sodium formate is 1:0.33-1.0, and the concentration of 2-methylimidazole is 0.05-0.2 mol / L.
[0013] As a further optimization of the above technical solution, the volume ratio of ammonia water to methanol in step S2 is 2-3:100.
[0014] As a further optimization of the above technical solution, the reaction time at room temperature in step S3 is 6-24 hours.
[0015] As a further optimization of the above technical solution, after the reaction is allowed to stand at room temperature in step S3, it is washed with deionized water and methanol respectively, then placed in chloroform for activation, taken out and dried at 60-80°C to obtain a ZIF-8 film.
[0016] A ZIF-8 film is prepared by adopting the method of in-situ conversion of the zinc-plated layer into the ZIF-8 film.
[0017] An SPME probe comprises a metal carrier and a ZIF-8 film attached to the metal carrier, wherein the metal carrier is a stainless steel wire, an aluminum wire, a copper wire or a nickel-titanium alloy wire, and the ZIF-8 film is a ZIF-8 film prepared by the above method.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention utilizes an electrochemical method to prepare a zinc coating on a metal carrier, and the thickness and density of the zinc coating are precisely controlled by adjusting the voltage and time. The thickness and density of the zinc coating are correlated with the thickness of the ZIF-8 film formed by the in-situ conversion thereof. Based on the different thicknesses of the zinc coating, ZIF-8 films of different thicknesses can be prepared. Therefore, the present invention can accurately control the ZIF-8 film by adjusting the thickness of the zinc coating.
[0020] The present invention converts the zinc-plated layer on the metal carrier into a ZIF-8 film in situ, and there is no need to fix the ZIF-8 film on the carrier by a sol-gel method, an adhesive method, etc., thereby avoiding the clogging of ZIFs pores by the sol during the process of fixing the ZIF-8 film; and the use of a metal wire as a metal carrier of the SPME probe has a higher mechanical strength.
[0021] The method provided by the present invention only requires an ordinary glass bottle to complete the process except that an electrochemical workstation is required for zinc plating. There is no special requirement for instruments and equipment, and batch preparation is possible. The zinc plating layer on the metal carrier is in situ converted into a ZIF-8 film, and there is no need to prepare ZIF-8 in advance, and the reagent consumption is small. The zinc plating layer is in situ converted into ZIF-8 under ambient conditions (room temperature, normal pressure, and no stirring required), and the conversion solution can be reused dozens of times, with low reagent consumption and low cost.
[0022] 2. The present invention prepares ZIF-8 thin film based on a technical concept different from the prior art, enriching the preparation path of ZIF-8 thin film and SPME probe. The present invention converts the zinc coating layer into ZIF-8 thin film in situ under room temperature, normal pressure and non-stirring environmental conditions, without adding an oxidant or special instruments and equipment. In the process of forming a zinc coating layer on a metal carrier and converting the zinc coating layer into ZIF-8 thin film in situ, ammonia water reacts with amphoteric metal zinc to obtain divalent zinc ions, and then the divalent zinc ions and ammonia water form zinc-ammine complexes, and finally the zinc-ammine complexes react with deprotonated ligands to obtain ZIF-8. The prepared ZIF-8 thin film has a long service life, good stability and high extraction efficiency, and can meet the requirements of trace analysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 XRD diagrams of ZIF-8 prepared by the present invention and simulated ZIF-8;
[0024] Figure 2 The infrared spectra of ZIF-8 and 2-methylimidazole prepared by the present invention;
[0025] Figure 3 SEM images (high magnification) of ZIF-8 generated for different zinc coating conversion times (A: 3 h; B: 6 h; C: 12 h; D: 24 h);
[0026] Figure 4 The SEM images of stainless steel wire before and after galvanizing, where A is the stainless steel wire after the zinc layer is scraped off, and B is the stainless steel wire coated with zinc layer;
[0027] Figure 5 This is the SEM image of the ZIF-8 film transformed from the zinc coating (low magnification);
[0028] Figure 6 This is the chromatogram of the SPME probe extraction of 10 μg / L polycyclic aromatic hydrocarbons in aqueous solution, including 1-naphthalene; 2-acenaphthylene; 3-acenaphthene; 4-fluorene; 5-anthracene; 6-phenanthrene; 7-fluoranthene; and 8-pyrene. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further elaborated in detail below in conjunction with specific embodiments. The parts of the present invention that are not described and disclosed in detail in the following embodiments should be understood as the prior art known or should be known to those skilled in the art.
[0030] The present invention discloses a method for in-situ converting a zinc coating into a ZIF-8 film, comprising the following steps:
[0031] S1: Preparation of zinc coating on metal support
[0032] Specifically: first, the metal carrier is ultrasonically cleaned with ethanol and deionized water respectively to remove any contaminants that may exist on its surface, and then dried in air. Then, the metal carrier is used as a working electrode, a saturated calomel electrode is used as a reference electrode, a platinum wire is used as a counter electrode, and an aqueous solution of zinc sulfate is used as an electrolyte. A certain voltage and time are controlled to electroplate a zinc layer of a required thickness on the metal carrier to obtain a zinc-plated layer. The metal carrier is a stainless steel wire, an aluminum wire, a copper wire, a nickel-titanium alloy wire, a metal plate or a blank SPME arrow.
[0033] S2: Prepare the conversion solution
[0034] Dissolving 2-methylimidazole and sodium formate in methanol, and then adding ammonia water to obtain a conversion solution, wherein the molar ratio of 2-methylimidazole to sodium formate in the conversion solution is 1:0.33-1.0, the concentration of 2-methylimidazole is 0.05-0.2 mol / L; the volume ratio of ammonia water to methanol is 2-3:100; wherein 2-methylimidazole is a ligand and sodium formate is a deprotonating agent;
[0035] S3: Preparation of ZIF-8 thin films
[0036] The metal support with the zinc-plated layer in step S1 is immersed in the conversion solution prepared in step S2, and allowed to react at room temperature for 6-24 hours to in-situ convert the zinc-plated layer into a ZIF-8 film;
[0037] S301: soaking the metal support with the zinc coating in step S1 in the conversion solution prepared in step S2, and standing at room temperature for 6-24 hours. During this process, ammonia water can react with amphoteric metal zinc to obtain divalent zinc ions, and then the divalent zinc ions and ammonia water form zinc-ammine complexes, and finally the zinc-ammine complexes react with the deprotonated ligands to obtain ZIF-8;
[0038] S302: After the reaction is completed, the metal carrier is taken out, rinsed with deionized water to remove the unreacted ligands and deprotonating agents that may be attached to the film, and then washed with methanol. Finally, it is immersed in chloroform for 8-12 hours to activate the ZIF-8 film, exchange the methanol in the ZIF-8 pores, shorten the subsequent drying time, and dry the activated metal carrier at a temperature of 60-80°C for 8-12 hours to obtain the ZIF-8 film, which is attached to the metal carrier.
[0039] The present invention also discloses an SPME probe, which comprises a metal carrier and a ZIF-8 film attached to the metal carrier. The metal carrier of the SPME probe is a stainless steel wire, an aluminum wire, a copper wire, a nickel-titanium alloy wire or other conductive metal wires, and the ZIF-8 film is a ZIF-8 film obtained by the above-mentioned method of in-situ conversion of a zinc-plated layer into a ZIF-8 film.
[0040] When the ZIF-8 film is prepared by the above-mentioned method of in-situ conversion of the zinc-plated layer into ZIF-8, the metal carrier is selected as stainless steel wire, aluminum wire, copper wire, nickel-titanium alloy wire or other conductive metal wire, and the obtained metal wire loaded with the ZIF-8 film constitutes the SPME probe.
[0041] The SPME probe of the present invention has good enrichment ability for non-polar organic matter, and when used in conjunction with GC / HPLC, it can be used for quantitative analysis of organic pollutants in environmental samples (including air, water samples, etc.). The stability of the film and the reproducibility of the preparation meet the relevant requirements of the SPME technology.
[0042] The SPME probe described in this method has a simple preparation method. When commercial galvanized wire is used, no special instruments or equipment are required, and only a few glass bottles are needed to complete the process. This method is carried out under ambient conditions (room temperature and normal pressure), has the advantages of simple operation, easy availability of required equipment, low cost (the conversion solution can be reused dozens of times), and batch preparation. ZIF-8 films can also be prepared on galvanized metal plates or galvanized materials of any shape, and has certain promotion value.
[0043] Example 1
[0044] A method for in-situ conversion of a zinc coating into a ZIF-8 film comprises the following steps:
[0045] S1: Preparation of zinc coating on metal support
[0046] S101: Pretreatment of carrier
[0047] A 304 stainless steel wire with a diameter of 0.15 mm was ultrasonically cleaned with ethanol and deionized water for 10 min respectively to remove any contaminants that might exist on its surface, and then dried in air.
[0048] S102: Preparation of zinc coating
[0049] In a 10mL weighing bottle, add 0.2mol / L zinc sulfate / water solution (0.575g zinc sulfate heptahydrate, dissolved in 10mL deionized water), use a stainless steel wire with a diameter of 0.15mm as the working electrode, a saturated calomel electrode as the reference electrode, a platinum wire (diameter of 0.4mm) as the counter electrode, the voltage is -1.4V, and the deposition time is 120 seconds to obtain galvanized stainless steel wire.
[0050] S2: Preparation of transformation solution
[0051] Weigh 0.082 g of 2-methylimidazole and 0.068 g of sodium formate, dissolve them in 10 mL of methanol, sonicate to completely dissolve them, and then add 0.2 mL of concentrated aqueous ammonia to obtain a conversion solution (the molar ratio of the ligand to the deprotonating agent is 1:1, the concentration of the ligand is 0.1 mol / L, and the volume ratio of aqueous ammonia to methanol is 2:100).
[0052] S3: Preparation of ZIF-8 thin films
[0053] The galvanized stainless steel wire was immersed in the conversion solution and allowed to react at room temperature for 24 hours to obtain a ZIF-8 film on the stainless steel wire. After the reaction was completed, the stainless steel wire was taken out, washed with deionized water and methanol respectively, and then immersed in chloroform overnight (activation, exchange of methanol in the ZIF-8 pores, shortening the drying time). The stainless steel wire was taken out and dried in an oven at 60°C overnight to obtain the ZIF-8 film.
[0054] The stainless steel wire with the ZIF-8 film obtained in this embodiment is the SPME probe.
[0055] Example 2
[0056] Step S1 of this embodiment is consistent with step S1 of embodiment 1, except that:
[0057] S2: Preparation of transformation solution
[0058] Weigh 0.123 g of 2-methylimidazole and 0.068 g of sodium formate, dissolve them in 10 mL of methanol, and sonicate to completely dissolve them. Then add 0.3 mL of concentrated aqueous ammonia to obtain a conversion solution (the molar ratio of the ligand to the deprotonating agent is 1:0.66, the concentration of the ligand is 0.15 mol / L, and the volume ratio of aqueous ammonia to methanol is 3:100).
[0059] S3: Preparation of ZIF-8 thin films
[0060] The galvanized stainless steel wire was immersed in the conversion solution and allowed to react at room temperature for 12 hours to obtain a ZIF-8 film on the stainless steel wire. After the reaction was completed, the stainless steel wire was taken out, washed with deionized water and methanol respectively, and then immersed in chloroform overnight (activation, exchange of methanol in the ZIF-8 pores, shortening the drying time). The stainless steel wire was taken out and dried in an oven at 80°C overnight to obtain the ZIF-8 film.
[0061] The stainless steel wire with the ZIF-8 film obtained in this embodiment is the SPME probe.
[0062] Example 3
[0063] Step S1 of this embodiment is consistent with step S1 of embodiment 1, except that:
[0064] S2: Preparation of transformation solution
[0065] Weigh 0.184 g of 2-methylimidazole and 0.136 g of sodium formate, dissolve them in 10 mL of methanol, sonicate to completely dissolve them, and then add 0.3 mL of concentrated aqueous ammonia to obtain a conversion solution (the molar ratio of the ligand to the deprotonating agent is 1:1, the concentration of the ligand is 0.2 mol / L, and the volume ratio of aqueous ammonia to methanol is 3:100).
[0066] S3: Preparation of ZIF-8 thin films
[0067] The galvanized stainless steel wire was immersed in the conversion solution and allowed to react at room temperature for 6 hours to obtain a ZIF-8 film on the stainless steel wire. After the reaction was completed, the stainless steel wire was taken out, washed with deionized water and methanol respectively, and then immersed in chloroform overnight (activation, exchange of methanol in the ZIF-8 pores, shortening the drying time). The stainless steel wire was taken out and dried in an oven at 65°C overnight to obtain the ZIF-8 film.
[0068] The stainless steel wire with the ZIF-8 film obtained in this embodiment is the SPME probe.
[0069] Comparative Example 1
[0070] The steps of this comparative example are generally the same as those of Example 1, except that:
[0071] S2: Preparation of transformation solution
[0072] Weigh 0.082 g of 2-methylimidazole and 0.101 g of triethylamine (deprotonating agent), dissolve them in 10 mL of methanol, sonicate to completely dissolve them, and then add 0.2 mL of concentrated aqueous ammonia to obtain a conversion solution.
[0073] The other steps are the same as in Example 1 to obtain a ZIF-8 film attached to a stainless steel wire.
[0074] Comparative Example 2
[0075] The steps of this comparative example are generally the same as those of Example 1, except that:
[0076] S2: Preparation of transformation solution
[0077] Weigh 0.082 g of 2-methylimidazole and 0.068 g of sodium formate, dissolve them in 10 mL of methanol, and sonicate to completely dissolve them to obtain a conversion solution.
[0078] The other steps are the same as in Example 1 to obtain a ZIF-8 film attached to a stainless steel wire.
[0079] Comparative Example 3
[0080] This comparative example is generally the same as the steps of Example 1, the difference is that:
[0081] S2: Preparation of the conversion solution
[0082] Weigh 0.082 g of 2-methylimidazole and 0.068 g of sodium formate, dissolve them in 10 mL of water, and ultrasonically dissolve them completely. Then add 0.2 mL of concentrated ammonia water to obtain the conversion solution.
[0083] Other steps are the same as those in Example 1 to obtain the ZIF-8 film attached to the stainless steel wire.
[0084] Comparative Example 4
[0085] This comparative example is generally the same as the steps of Example 1, the difference is that:
[0086] S2: Preparation of the conversion solution
[0087] Weigh 0.082 g of 2-methylimidazole and 0.068 g of sodium formate, dissolve them in 10 mL of methanol, and ultrasonically dissolve them completely. Then add 0.2 mL of hydrogen peroxide as an oxidant to obtain the conversion solution. Other steps are the same as those in Example 1 to obtain the ZIF-8 film attached to the stainless steel wire.
[0088] Next, the ZIF-8 film and the SPME probe obtained in Example 1 are detected and analyzed:
[0089] <Characterization of the ZIF-8 film>
[0090] The ZIF-8 film prepared in Example 1 of the present invention is characterized by a scanning electron microscope (SEM), an X-ray diffractometer (XRD), and a Fourier transform infrared spectrometer (FT-IR) to confirm the formation of ZIF-8.
[0091] I. XRD pattern of the ZIF-8 film prepared by the present invention
[0092] As Figure 1 shown is the XRD pattern of the ZIF-8 film prepared by the present invention. After scraping off the film prepared by the present invention, its crystal structure is detected by an X-ray diffractometer. The main diffraction peaks of the XRD of the ZIF-8 prepared by this method are basically consistent with the positions of the simulated diffraction peaks of ZIF-8, indicating that the galvanized layer has been successfully converted into ZIF-8.
[0093] II. FT-IR pattern of the ZIF-8 film
[0094] After scraping the ZIF-8 film prepared by this method from the stainless steel wire, its infrared spectrum was measured by the potassium bromide tablet method ( Figure 2), which is consistent with the main adsorption peaks in the infrared spectrum of ZIF-8 prepared in the prior art. In the infrared spectrum of ZIF-8 prepared in the present invention, the stretching vibration absorption peak of the N-H bond of 2-methylimidazole (~1842 cm -1 ) disappears, while a strong stretching vibration absorption peak of the Zn-N bond appears at 421 cm -1 (Microporous and Mesoporous Materials, 2014, 184: 55-60), further proving the successful preparation of ZIF-8.
[0095] III. Scanning Electron Microscope Characterization
[0096] To observe the microstructures of the prepared galvanized layer and ZIF-8, their apparent structures were observed using a scanning electron microscope (SEM). As can be seen from Figure 3 A, when the conversion time is 24 hours, most of the prepared ZIF-8 is in the form of rhombic dodecahedrons, and the crystal size is between 0.5 - 1 μm. While when the conversion time is 12 hours, the crystal size is between 0.1 - 0.5 μm ( Figure 3 B), and most of the crystals are cubes, and there are significant differences in the crystal particle sizes. The reason for this phenomenon may be that with the extension of the standing time, Ostwald ripening occurs, that is, the smaller ZIF-8 crystals in the conversion film will dissolve and redeposit on the larger crystals, thus changing the main form from cubes to the more thermodynamically stable dodecahedrons. For the films prepared with a conversion time of 3 - 6 hours, ZIF-8 mainly exists in the form of nanoparticles, and there are pores between the particles ( Figure 3 C, D). Although its extraction efficiency has no significant difference from that of the conversion for 12 - 24 hours, due to the non-dense film, the film may fall off after multiple extractions, affecting its service life.
[0097] Measured by SEM, the diameter of the stainless steel wire plated with a zinc layer is 163 μm ( Figure 4 -B), and the diameter after scraping off the zinc layer is 153 μm ( Figure 4 -A), that is, the thickness of the galvanized layer is about 10 μm. The density of zinc is 7.14 g / cm 3 , while the density of ZIF-8 is 0.93 g / cm 3 . Theoretically, after the galvanized layer is converted to ZIF-8, the thickness of the ZIF-8 film should be 7.6 times the thickness of the galvanized layer, that is, it should be 76 μm. The actual measured thickness of the ZIF-8 film is 67 μm, which is relatively close to the theoretically calculated value ( Figure 5 ), thus it can be proved that by controlling the thickness of the galvanized layer during electroplating, the thickness of the ZIF-8 film can be controlled.
[0098] <Performance Investigation of SPME Probe>
[0099] Assembly of the SPME extraction device: Use a 1 mL disposable medical syringe, a spotting needle with an inner diameter of 0.40 mm (outer diameter of 0.65 mm), a stainless steel capillary with an inner diameter of 0.15 mm, and a silicone pad to make a homemade SPME handle (for specific methods, see patent: ZL202320721040.X), and then assemble the prepared SPME probe on the SPME handle to obtain the SPME device, and examine the extraction performance of the probe through extraction tests.
[0100] 1. Before the extraction experiment, the SPME probe was aged at 280°C for more than 60 min at the gas chromatography injection port to remove impurities that may be adsorbed on the probe.
[0101] 2. Extraction experiments were carried out using aqueous solutions of 8 PAHs (naphthalene, acenaphthylene, acenaphthene, fluorene, anthracene, phenanthrene, fluoranthene, and pyrene) at a concentration of 10 μg / L as simulated targets.
[0102] 3. Extraction conditions: 20mL headspace bottle, 5-15mL PAH aqueous solution, with or without inorganic salt, extraction temperature 60-80℃, time 30-60min, stirring speed 800rpm. Extraction mode: headspace extraction.
[0103] 4. Chromatographic analysis conditions: The separation of the target was carried out on a HP-5 (30m×250μm×0.25μm) capillary column. The column box was programmed to heat: the initial temperature was 50°C (maintained for 5min), then increased to 250°C at 10°C / min (maintained for 2min). Inlet temperature: 280°C, column head pressure: 12.2psi; non-split injection, desorption time was 5min. FID detector conditions: temperature was 300°C; carrier gas was high-purity nitrogen (99.999%); hydrogen flow rate was 35mL / min; air flow rate was 300mL / min.
[0104] 1. Investigation of the stability of the SPME probe
[0105] In order to evaluate the stability of the SPME probe prepared by the method of in-situ conversion of the zinc coating into the ZIF-8 film of the present invention, 30 extraction and GC analysis experiments were carried out continuously with the same SPME probe during the test [5 mL of a polycyclic aromatic hydrocarbon aqueous solution with a concentration of 10 μg / L; extraction temperature of 60°C; extraction time of 30 min; no salt added; stirring speed of 800 rpm; desorption time of 5 min], and the results are shown in Table 2.
[0106] Table 2 Stability of prepared ZIF-8 films
[0107] It can be seen from Table 2 that the SPME probe of the ZIF-8 film prepared by this method has no significant change in extraction efficiency after 30 consecutive extractions, and the relative standard deviation (RSD%) of the three analysis results is between 1.6% and 25.7%. Except for the large relative standard deviation of naphthalene (due to the interference of impurity peaks, resulting in a large integral error), the RSD% of most analyses is less than 10%. This shows that the prepared probe has good stability and can meet the requirements of SPME analysis applications.
[0108] 2. Reproducibility of SPME probe
[0109] In order to test the reproducibility of this method, three SPME probes were made using the method of Example 1, and then an extraction experiment was carried out; then the same probe was used to repeat the extraction experiment 5 times [extraction conditions: 20mL headspace bottle, the volume of the analyte aqueous solution was 5mL, the concentration was 10μg / L, the extraction temperature was 60°C, the extraction time was 30min, the extraction mode was headspace extraction, no salt was added, the stirring speed was 800rpm, and the desorption time was 5min]. The test results are shown in Table 3:
[0110] Table 3 Reproducibility and reproducibility
[0111] As can be seen from Table 3, the relative standard deviation of the extraction results between probes is between 5.7% and 18.6%, and within the probe is between 5.0% and 18.5%, indicating that this method has good production reproducibility and can be reproduced in other laboratories.
[0112] 3. Extraction chromatogram
[0113] Figure 6 This is the chromatogram of the SPME probe extraction of 10 μg / L polycyclic aromatic hydrocarbons in aqueous solution, including 1-naphthalene; 2-acenaphthylene; 3-acenaphthene; 4-fluorene; 5-anthracene; 6-phenanthrene; 7-fluoranthene; and 8-pyrene.
[0114] Extraction conditions: 5 mL of 10 μg / L PAH aqueous solution, extraction temperature of 70°C, extraction time of 50 min, addition amount of sodium sulfate of 0.5 g, stirring speed of 800 rpm, desorption time of 5 min.
[0115] The extraction performance of the ZIF-8 film prepared in the comparative example and the ZIF-8 film prepared in Example 1 are compared below:
[0116] The difference between Comparative Example 1 and Example 1 is that triethylamine is used instead of sodium formate as a deprotonating agent, and the thickness of the obtained ZIF-8 film is thinner; the difference between Comparative Example 2 and Example 1 is that no ammonia water is added, and no hydrogen peroxide is added, and the zinc coating layer is not converted; the difference between Comparative Example 3 and Example 1 is that water is used instead of methanol as a solvent, and the obtained film is also thinner; the difference between Comparative Example 4 and Example 1 is that no ammonia water is added, but hydrogen peroxide is used as an oxidant, and the obtained film is also very thin. The results of the extraction of 8 kinds of polycyclic aromatic hydrocarbons by Comparative Example and Example 1 are shown in Table 1. Table 1 Comparison of extraction results between comparative example and embodiment 1
[0117] It can be seen from the above test data that if triethylamine is used instead of sodium formate (i.e., Comparative Example 1), the extraction efficiency of the prepared ZIF-8 film is lower than that of Example 1 except that fluoranthene and pyrene are equivalent to those of Example 1; if no ammonia water is added (i.e., Comparative Example 2) and no hydrogen peroxide is added, zero-valent zinc cannot react with the deprotonated ligand and the ZIF-8 film cannot be obtained; if the solvent methanol is replaced with water (i.e., Comparative Example 3), the extraction efficiency of the obtained ZIF-8 film is lower than that of Example 1 except that fluoranthene and pyrene are equivalent to those of Example 1; if hydrogen peroxide is used as an oxidant without adding ammonia water (i.e., Comparative Example 4), the extraction efficiency of the prepared ZIF-8 film for 8 polycyclic aromatic hydrocarbons is also lower than that of Example 1.
[0118] These experimental results show that in the experiment of in situ conversion of the zinc-coated layer into the ZIF-8 film, the conversion efficiency of the zinc-coated layer is relatively high when methanol is used as the solvent, sodium formate is used as the deprotonating agent, and ammonia water is used as the additive. This indicates that in the in situ conversion of the zinc-coated layer into the ZIF-8 film, the synergistic effect of ammonia water, methanol, and sodium formate ultimately leads to the preparation of the ZIF-8 film with high extraction efficiency and suitable for SPME coating.
[0119] In the preparation method of the present invention, sodium formate as a deprotonating agent has a positive effect on the generation of ZIF-8 with good crystal form, and the crystal form has an important influence on the stability of ZIF-8; the present invention chooses to use ammonia water instead of an oxidant, and ammonia water plays two roles here: one is that it can convert zero-valent zinc into divalent zinc ions; the second is that it can react with the formed zinc ions to generate a complex as an intermediate for the final formation of ZIF-8; in addition, the addition of ammonia water can accelerate the reaction rate, so that the reaction can be carried out at a lower temperature, and the ZIF-8 particles obtained by adding ammonia water are smaller, and the small particles have a larger specific surface area, thereby having a higher extraction efficiency.
[0120] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for in-situ conversion of a zinc coating into a ZIF-8 film, characterized in that: The following steps are included: S1: preparing a zinc coating on a metal support; S2: Mix 2-methylimidazole, sodium formate, methanol and aqueous ammonia to obtain a conversion solution; S3: Soak the metal support with the zinc-plated layer in step S1 in the conversion solution obtained in step S2, and allow the reaction to stand at room temperature to convert the zinc-plated layer into a ZIF-8 film in situ.
2. The method for in-situ conversion of a zinc coating into a ZIF-8 film according to claim 1, characterized in that: Step S1 specifically comprises: using a conductive metal carrier as a working electrode, a saturated calomel electrode as a reference electrode, a platinum wire as a counter electrode, and a zinc sulfate aqueous solution as an electrolyte, controlling voltage and time, and electroplating zinc on the metal carrier to obtain a zinc-plated layer.
3. The method for in-situ conversion of a zinc coating into a ZIF-8 film according to claim 1, characterized in that: The metal carrier is a stainless steel wire, an aluminum wire, a copper wire, a nickel-titanium alloy wire, a metal plate or a blank SPME arrow.
4. The method for in-situ conversion of a zinc coating into a ZIF-8 film according to claim 1, characterized in that: Before step S1, the method further comprises ultrasonically cleaning the metal carrier with ethanol and deionized water respectively.
5. The method for in-situ conversion of a zinc coating into a ZIF-8 film according to claim 1, characterized in that: In step S2, the molar ratio of 2-methylimidazole to sodium formate is 1:0.33-1.0, and the concentration of 2-methylimidazole is 0.05-0.2 mol / L.
6. The method for in-situ conversion of a zinc coating into a ZIF-8 film according to claim 1, characterized in that: The volume ratio of ammonia water to methanol in step S2 is 2-3:
100.
7. The method for in-situ conversion of a zinc coating into a ZIF-8 film according to claim 1, characterized in that: The reaction time at room temperature in step S3 is 6-24 hours.
8. The method for in-situ conversion of a zinc coating into a ZIF-8 film according to claim 1, characterized in that: In step S3, after the reaction is allowed to stand at room temperature, the film is washed with deionized water and methanol respectively, and then activated in chloroform. After being taken out, the film is dried at 60-80° C. to obtain a ZIF-8 film.
9. A ZIF-8 film, characterized in that The film is prepared by in-situ conversion of any one of the zinc-plated layers described in claims 1 to 8 into a ZIF-8 film.
10. An SPME probe, comprising a metal carrier and a ZIF-8 film attached to the metal carrier, wherein the metal carrier is a stainless steel wire, an aluminum wire, a copper wire or a nickel-titanium alloy wire, characterized in that: The ZIF-8 film is a ZIF-8 film according to claim 9.