Coating system for electrolytic cell for producing hydrogen by electrolyzing water and preparation method of coating system

By using a pre-floor layer and a metal mixed layer coating system in the electrolytic water hydrogen production cell, the corrosion problem of titanium-based materials in harsh environments is solved, the cost is reduced, and the conductivity and durability are improved to ensure coating The layer does not fall off at high potential, achieving a longer service life.

CN118979266APending Publication Date: 2024-11-19BEIJING SMART ENERGY RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411054450.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing titanium-based bipolar plates and porous transport layers are easily corroded under the harsh environment of electrolyzing hydrogen production, the cost of precious metal coatings is high, and the hybrid carbon coating is easily oxidized at high potentials, causing the coating to fall off, affecting the conductivity and Durability.

Method used

The pre-transfer layer and metal mixed layer coating system are adopted that adhere to the inside from the outside in sequence. The material of the pre-transfer layer is the same as the substrate. The metal mixed layer includes platinum, iridium, gold and transition metal. It is attached by magnetron sputtering method to ensure that The coating does not fall off under water flow and oxygen flush, and reduces costs.

Benefits of technology

It improves the conductivity, corrosion resistance and durability of the titanium bipolar plate and porous transport layer, keeps the coating from falling off, costs lower than that of precious metal coatings, and has a longer service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979266A_ABST
    Figure CN118979266A_ABST
Patent Text Reader

Abstract

The invention discloses a coating system for a water electrolysis hydrogen production electrolytic cell and a preparation method. The coating system comprises a pre-plating layer and a metal mixing layer which are sequentially connected and attached to the surface of a base material from inside to outside. The material of the pre-plated layer is the same as that of the base material; the metal mixing layer comprises a first metal and a second metal which are mixed with each other; the first metal is made of any one of platinum, iridium and gold; the second metal is made of transition metal. The coating system has the beneficial effects that the conductivity, the corrosion resistance and the durability of a matrix can be improved, the coating system does not fall off under the working condition, the cost is low, and the preparation method of the coating system for the electrolytic cell for hydrogen production through water electrolysis is simple, easy to implement and high in operability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogen production by water electrolysis, and in particular to a coating system and a preparation method of an electrolytic cell for hydrogen production by water electrolysis. Background Art

[0002] Titanium is the mainstream material for manufacturing bipolar plates and porous transport layers for hydrogen production by water electrolysis. It has excellent thermal conductivity, electrical conductivity, durability and chemical stability. However, in the actual working environment of water electrolysis for hydrogen production, titanium-based bipolar plates and porous transport layers still face harsh corrosion environments: high potential, oxygen-rich, high operating temperature, acidic environment, etc. Passivation is very easy to occur, which increases contact resistance and affects the durability and hydrogen production efficiency of the bipolar plate. Therefore, it is necessary to construct a coating system with good conductivity, strong corrosion resistance and long durability on the titanium substrate of the bipolar plate and porous transport layer. Existing coating systems for bipolar plates and porous transport layers include: (1) precious metal coatings mainly composed of platinum, iridium and gold; (2) metal-doped coatings, mainly doping metals with one or more elements of N, C, O, such as TiN, ZrC, TiCN, TiNO, etc.; (3) hybrid carbon coatings, directly constructing hybrid carbon coatings on bipolar plates and porous transport layers. The above method has the following problems: (1) Titanium-based bipolar plates and porous transport layers still face harsh corrosion environments: high potential, oxygen-rich, high operating temperature, acidic environment, and F ions. The resulting passivation, pitting and dissolution of titanium ions lead to increased contact resistance and contamination of the proton exchange membrane. (2) The high cost of precious metal coatings greatly restricts the development of the water electrolysis industry; (3) Under high current density, the bipolar plates and porous transport layers on the anode side will be continuously eroded by water and oxygen, which can easily cause the coating to fall off and fail; (4) The carbon in the hybrid carbon coating is easily oxidized under high potential conditions of water electrolysis to produce hydrogen, causing damage and failure of the coating. Summary of the invention

[0003] In order to solve the above-mentioned problems in the prior art, the present invention provides a coating system for an electrolytic cell for producing hydrogen by electrolysis of water, which improves the conductivity, corrosion resistance and durability of the substrate, does not fall off under working conditions, and has a low cost. At the same time, a simple, easy and highly operable preparation method of the coating system for an electrolytic cell for producing hydrogen by electrolysis of water is provided.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides a coating system for an electrolytic cell for producing hydrogen by electrolysis of water, comprising a pre-coating layer and a metal mixed layer which are sequentially attached to the surface of a substrate from the inside to the outside;

[0005] The material of the pre-coating layer is the same as that of the substrate;

[0006] The metal mixed layer includes a first metal and a second metal mixed with each other;

[0007] The material of the first metal is any one of platinum, iridium and gold; the material of the second metal is a transition metal.

[0008] Furthermore, the material of the pre-coating layer is titanium.

[0009] Furthermore, the molar ratio of the first metal to the second metal is (1-5):1.

[0010] Furthermore, the second metal is made of any one of zirconium, tantalum, niobium, molybdenum and tungsten.

[0011] Furthermore, the substrate is a bipolar plate or a porous transport layer in an electrolytic cell.

[0012] Furthermore, the pre-coating layer is attached to the surface of the substrate by a magnetron sputtering method, and the metal mixed layer is attached to the surface of the pre-coating layer by a magnetron sputtering method.

[0013] A method for preparing the coating system for the electrolytic cell for producing hydrogen by electrolysis of water comprises the following steps:

[0014] Performing pickling treatment on the substrate;

[0015] A first target material, a second target material and a third target material are respectively installed on the magnetron sputtering device, wherein the material of the first target material is the same as the material of the pre-sputtering layer, the material of the second target material is the same as the material of the first metal, and the material of the third target material is the same as the material of the second metal;

[0016] Placing the substrate on the substrate stage of the magnetron sputtering device, and heating the substrate to a temperature of 300° C. to 900° C.;

[0017] The pre-coating layer is firstly attached to the surface of the substrate by using the first target material, and then the metal mixed layer is attached to the surface of the pre-coating layer by using the second target material and the third target material.

[0018] Furthermore, the pickling step is:

[0019] Pickling the substrate with one or more of oxalic acid, hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid, performing a heating treatment during pickling, with a temperature range of 25° C. to 90° C. and a pickling time of 5 min to 2 h;

[0020] The pickled substrate was washed with deionized water for more than 3 times.

[0021] Furthermore, before heating the substrate, the surface of the substrate is bombarded with argon ions for 10 min to 30 min.

[0022] Furthermore, the first target, the second target and the third target are respectively connected to a DC power supply.

[0023] The beneficial effects of the present invention are:

[0024] 1. The present invention introduces a pre-coating made of the same material as the substrate, which can ensure that the coating does not fall off when the water flow and oxygen are constantly washed away. The presence of any one of platinum, iridium and gold can effectively improve the conductivity, corrosion resistance and durability of the titanium bipolar plate and the porous transmission layer for electrolyzing water to produce hydrogen. At the same time, the metal mixed layer formed by mixing any one of platinum, iridium and gold with transition metals has a lower cost than the precious metal coating and has a significantly longer service life than the non-precious metal coating;

[0025] 2. The coating system provided by the present invention has high electrical conductivity and corrosion resistance;

[0026] 3. The coating system provided by the present invention ensures that the coating system does not fall off under the flushing of water flow and oxygen under working conditions;

[0027] 4. The preparation method of the coating system provided by the present invention is simple and easy to implement, and has strong operability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Polarization curves of titanium substrates having coating systems of Example 1, Example 2, and Example 3 of the present invention and a titanium substrate of a comparative example;

[0029] Figure 2 The graph is a graph showing the contact resistance of the titanium substrate having the coating system of Example 1, Example 2, and Example 3 of the present invention as a function of pressure. DETAILED DESCRIPTION

[0030] In order to clearly illustrate the technical features of this solution, this solution is described below through a specific implementation method.

[0031] The embodiment of the present invention provides a coating system for an electrolytic cell for producing hydrogen by electrolysis of water, comprising a pre-coating layer and a metal mixed layer sequentially attached to the surface of a substrate from the inside to the outside; preferably, the substrate is a bipolar plate or a porous transport layer in the electrolytic cell;

[0032] The material of the pre-coating layer is the same as that of the substrate; preferably, the thickness of the pre-coating layer is greater than or equal to 5 nm and less than 1 μm;

[0033] The metal mixed layer includes a first metal and a second metal mixed with each other; preferably, the thickness of the metal mixed layer is 100 nm;

[0034] The material of the first metal is any one of platinum, iridium and gold; the material of the second metal is a transition metal.

[0035] Introducing a pre-coating made of the same material as the substrate can ensure that the coating does not fall off when constantly flushed by water and oxygen. The presence of any one of platinum, iridium, and gold can effectively improve the conductivity, corrosion resistance, and durability of the titanium bipolar plate and porous transport layer for electrolyzing water to produce hydrogen. At the same time, the metal mixed layer formed by mixing any one of platinum, iridium, and gold with transition metals has a lower cost than precious metal coatings and has a significantly longer service life than non-precious metal coatings.

[0036] In some preferred embodiments, the material of the pre-coating is titanium. Titanium, as the mainstream substrate for manufacturing bipolar plates and porous transport layers for hydrogen production by electrolysis of water, has excellent thermal conductivity and electrical conductivity, as well as excellent durability and chemical stability. Choosing titanium to make the pre-coating can not only have better bonding with the bipolar plate and the porous transport layer substrate, but also ensure that the coating system does not fall off when continuously flushed by water and oxygen.

[0037] In some preferred embodiments, the molar ratio of the first metal to the second metal is (1-5):1.

[0038] In some preferred embodiments, the material of the second metal is any one of zirconium, tantalum, niobium, molybdenum, and tungsten. On the pre-plated layer, any one of platinum, iridium, and gold is uniformly mixed with any one of zirconium, tantalum, niobium, molybdenum, and tungsten in a certain proportion to form a metal mixed layer, that is, the pre-plated layer and the metal mixed layer are sequentially prepared on the surface of the substrate to form a coating system, so that the substrate with the coating system can withstand harsh working conditions. Although a certain degree of passivation will occur over a long period of time, the contact resistance can still be maintained within an acceptable range, which has a certain guarantee for hydrogen production performance and efficiency.

[0039] In some preferred embodiments, the pre-coating layer is attached to the surface of the substrate by magnetron sputtering, and the metal mixed layer is attached to the surface of the pre-coating layer by magnetron sputtering.

[0040] A method for preparing a coating system for an electrolytic cell for producing hydrogen by electrolysis of water comprises the following steps:

[0041] The substrate is pickled;

[0042] In some preferred embodiments, the pickling step is:

[0043] Use one or more of oxalic acid, hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid to pickle the substrate, and perform heating treatment during pickling, with a temperature range of 25°C to 90°C and a pickling time of 5 minutes to 2 hours;

[0044] The pickled substrate was washed with deionized water for more than 3 times and then blown dry.

[0045] A first target material, a second target material and a third target material are respectively installed on the magnetron sputtering device, wherein the material of the first target material is the same as that of the pre-sputtering layer, preferably titanium, the material of the second target material is the same as that of the first metal, preferably any one of platinum, iridium and gold, and the material of the third target material is the same as that of the second metal, preferably any one of zirconium, tantalum, niobium, molybdenum and tungsten;

[0046] The substrate is placed on a substrate stage of a magnetron sputtering device, and heated to a temperature of 300° C. to 900° C.;

[0047] First, a pre-coating layer is attached to the surface of the substrate through the first target material, and then a metal mixed layer is attached to the surface of the pre-coating layer through the second target material and the third target material.

[0048] In some preferred embodiments, before heating the substrate, the substrate surface is bombarded with argon ions for 10 to 30 minutes to remove the oxide film remaining on the surface. After the oxide film is removed, the substrate is heated, and then the pre-coating layer is attached to the substrate surface through the first target material to achieve full contact between the pre-coating layer and the substrate.

[0049] In some preferred embodiments, the first target material, the second target material and the third target material are respectively connected to a DC power supply, wherein the first target material is connected to the DC power supply for DC sputtering to form a uniform pre-sputtering layer on the surface of the substrate, and the second target material and the third target material are connected to the DC power supply, and the parameters of the DC power supply are adjusted to make the first metal and the second metal uniformly mixed to form a metal mixed layer.

[0050] Specifically, when the pre-sputtering layer is attached to the surface of the substrate by the first target material, the power of the DC sputtering is 300W to 800W, and the sputtering time is 5min to 60min;

[0051] When a metal mixed layer is attached to the surface of the pre-coat layer through the second target and the third target, the ratio of the first metal to the second metal is adjusted by adjusting the DC sputtering power and the sputtering time. The power range of the DC sputtering of the second target and the third target is 200W to 1000W, and the sputtering time is 5min to 360min.

[0052] For ease of description, in the following embodiments or control examples, a substrate made of titanium is referred to as a titanium substrate, a pre-coating layer made of titanium is referred to as a titanium pre-coating layer, and a metal mixed layer prepared by mixing platinum and tantalum is referred to as a platinum-tantalum metal mixed layer.

[0053] Example 1

[0054] A coating system for an electrolytic cell for producing hydrogen by electrolysis of water, comprising a titanium pre-coating layer attached to a surface of a substrate, and a platinum-tantalum metal mixed layer attached to the surface of the titanium pre-coating layer, wherein the molar ratio of tantalum to platinum in the platinum-tantalum metal mixed layer is 1:1;

[0055] The preparation method comprises the following steps:

[0056] The titanium substrate is pickled; the steps of the pickling treatment are:

[0057] The titanium substrate is pickled using one or more of oxalic acid, hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid, and a heating treatment is performed during pickling, the heating temperature is 80°C, and the pickling time is 30 minutes;

[0058] The pickled titanium substrate was washed with deionized water for more than 3 times.

[0059] A titanium target, a platinum target and a tantalum target are respectively installed on the magnetron sputtering equipment, and the titanium target, the platinum target and the tantalum target are respectively connected to a DC power supply;

[0060] The titanium substrate was placed on the substrate stage of the magnetron sputtering equipment, the surface of the titanium substrate was bombarded with argon ions for 20 minutes, and then the substrate was heated to a temperature of 400°C;

[0061] First, a titanium pre-layer is attached to the surface of the titanium substrate through a titanium target. The power of DC sputtering of the titanium target is 500W, and the sputtering time is 10 minutes.

[0062] Then, a metal mixed layer is attached to the surface of the titanium pre-coat layer through a platinum target and a tantalum target: the DC sputtering power of the platinum target is 500 W, the DC sputtering power of the tantalum target is 500 W, and the sputtering time is 30 minutes.

[0063] Example 2

[0064] A coating system for an electrolytic cell for producing hydrogen by electrolyzing water, comprising a titanium pre-coating layer attached to a substrate surface, and a platinum-tantalum metal mixed layer attached to the surface of the titanium pre-coating layer, wherein the molar ratio of tantalum to platinum in the platinum-tantalum metal mixed layer is 1:3;

[0065] The preparation method comprises the following steps:

[0066] The titanium substrate is pickled; the steps of the pickling treatment are:

[0067] The titanium substrate is pickled using one or more of oxalic acid, hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid, and a heating treatment is performed during pickling, the heating temperature is 90°C, and the pickling time is 20 minutes;

[0068] The pickled titanium substrate was washed with deionized water for more than 3 times.

[0069] A titanium target, a platinum target and a tantalum target are respectively installed on the magnetron sputtering equipment, and the titanium target, the platinum target and the tantalum target are respectively connected to a DC power supply;

[0070] The titanium substrate was placed on the substrate stage of the magnetron sputtering equipment, the surface of the titanium substrate was bombarded with argon ions for 25 minutes, and then the substrate was heated to a temperature of 500°C;

[0071] First, a titanium pre-layer is attached to the surface of the titanium substrate through a titanium target. The power of DC sputtering of the titanium target is 400W, and the sputtering time is 15 minutes.

[0072] Then, a metal mixed layer is attached to the surface of the titanium pre-coat layer through a platinum target and a tantalum target: the DC sputtering power of the platinum target is 900 W, the DC sputtering power of the tantalum target is 300 W, and the sputtering time is 15 minutes.

[0073] Example 3

[0074] A coating system for an electrolytic cell for producing hydrogen by electrolyzing water, comprising a titanium pre-coating layer attached to a substrate surface, and a platinum-tantalum metal mixed layer attached to the surface of the titanium pre-coating layer, wherein the molar ratio of tantalum to platinum in the platinum-tantalum metal mixed layer is 1:5;

[0075] The preparation method comprises the following steps:

[0076] The titanium substrate is pickled; the steps of the pickling treatment are:

[0077] The titanium substrate is pickled using one or more of oxalic acid, hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid, and a heating treatment is performed during pickling, the heating temperature is 90°C, and the pickling time is 25 minutes;

[0078] The pickled titanium substrate was washed with deionized water for more than 3 times.

[0079] A titanium target, a platinum target and a tantalum target are respectively installed on the magnetron sputtering equipment, and the titanium target, the platinum target and the tantalum target are respectively connected to a DC power supply;

[0080] The titanium substrate was placed on the substrate stage of the magnetron sputtering equipment, the surface of the titanium substrate was bombarded with argon ions for 30 minutes, and then the substrate was heated to a temperature of 400°C;

[0081] First, a titanium pre-layer is attached to the surface of the titanium substrate through a titanium target. The power of DC sputtering of the titanium target is 500W, and the sputtering time is 10 minutes.

[0082] Then, a metal mixed layer is attached to the surface of the titanium pre-coat layer through a platinum target and a tantalum target: the DC sputtering power of the platinum target is 1000W, the DC sputtering power of the tantalum target is 200W, and the sputtering time is 15 minutes.

[0083] The titanium substrates with the coating systems of Example 1, Example 2, and Example 3, respectively, and the titanium substrate without any coating of the control example were subjected to a simulated PEMWE (proton exchange membrane electrolysis water) environmental test. The test conditions were a sulfuric acid solution with a pH of 3 and a fluoride ion concentration of 5 ppm. The test was carried out at a maintenance temperature of 75°C. The H2SO4 solution was prepared using distilled water and analytically pure chemicals. Before starting the electrochemical test, an open circuit potential measurement was performed for 1 hour. The polarization curve is shown in Figure 1 It can be seen that the titanium substrates having the coating systems of Example 1, Example 2, and Example 3 have lower corrosion current density and higher corrosion potential than the titanium substrate without any coating in the control example, and have better corrosion resistance than the titanium substrate without any coating in the control example.

[0084] The contact resistance values ​​(ICR) of the coating systems of Example 1, Example 2 and Example 3 under different pressures are shown in Figure 2 The results show that the contact resistance of the coating systems of Example 1, Example 2, and Example 3 does not change much under the same pressure. Under a pressure of 2MPa, the contact resistance values ​​are all <2mΩ·cm 2 , proving that the coating systems of Example 1, Example 2, and Example 3 have good electrical conductivity.

[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A coating system for an electrolytic cell for producing hydrogen by electrolysis of water, characterized in that: It includes a pre-coating layer and a metal mixed layer which are sequentially attached to the surface of the substrate from the inside to the outside; The material of the pre-coating layer is the same as that of the substrate; The metal mixed layer includes a first metal and a second metal mixed with each other; The material of the first metal is any one of platinum, iridium and gold; the material of the second metal is a transition metal.

2. The coating system for the electrolytic cell for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The material of the pre-coating layer is titanium.

3. The coating system for the electrolytic cell for producing hydrogen by electrolysis of water according to claim 1 or 2, characterized in that: The molar ratio of the first metal to the second metal is (1-5):

1.

4. The coating system for the electrolytic cell for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The second metal is made of any one of zirconium, tantalum, niobium, molybdenum and tungsten.

5. The coating system for the electrolytic cell for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The substrate is a bipolar plate or a porous transport layer in an electrolytic cell.

6. The coating system for the electrolytic cell for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The pre-coating layer is attached to the surface of the substrate by a magnetron sputtering method, and the metal mixed layer is attached to the surface of the pre-coating layer by a magnetron sputtering method.

7. A method for preparing a coating system for an electrolytic cell for producing hydrogen by electrolysis of water according to any one of claims 1 to 6, characterized in that: The following steps are involved: Performing pickling treatment on the substrate; A first target material, a second target material and a third target material are respectively installed on the magnetron sputtering device, wherein the material of the first target material is the same as the material of the pre-sputtering layer, the material of the second target material is the same as the material of the first metal, and the material of the third target material is the same as the material of the second metal; Placing the substrate on the substrate stage of the magnetron sputtering device, and heating the substrate to a temperature of 300° C. to 900° C.; The pre-coating layer is firstly attached to the surface of the substrate by using the first target material, and then the metal mixed layer is attached to the surface of the pre-coating layer by using the second target material and the third target material.

8. The preparation method according to claim 7, characterized in that: The steps of the pickling treatment are: Pickling the substrate with one or more of oxalic acid, hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid, performing a heating treatment during pickling, with a temperature range of 25° C. to 90° C. and a pickling time of 5 min to 2 h; The pickled substrate was washed with deionized water for more than 3 times.

9. The preparation method according to claim 7 or 8, characterized in that: Before heating the substrate, the surface of the substrate is bombarded with argon ions for 10 min to 30 min.

10. The preparation method according to claim 7, characterized in that: The first target, the second target and the third target are respectively connected to a direct current power supply.