Rodlike / hexagonal flaky Co (OH) 2 nano composite structure and preparation and application thereof

Co(OH)2 is reconstructed on the foam nickel/CoP/Co-MOF composite structure through electrochemical scanning technology, solving the problem of insufficient electrochemical activity in the existing Co(OH)2 nanostructure synthesis method, and the excellent preparation Electrochemical properties of rod-shaped/hexagonal sheet-shaped nanocomposite structure.

CN118979271APending Publication Date: 2024-11-19LIAONING INST OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068832.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing synthesis methods of Co(OH)2 nanostructures mainly rely on chemical precipitation method and etching method of MOF templates, and lack of electrochemical regulation methods, resulting in insufficient electrochemical activity and performance.

Method used

Using foam nickel/CoP/Co-MOF composite structure as working electrode, electrochemical scanning is performed in alkaline solution, and the conical CoP and Co-MOF block structures are electrochemically reconstituted to prepare rod-shaped/hexagonal sheet-shaped Co(OH)2 nanocomposite structure.

Benefits of technology

The electrochemical activity and performance of electrode materials has been improved. Through the integration of composite structures, the combination of fast ion transport characteristics and high-active surfaces has been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979271A_ABST
    Figure CN118979271A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of inorganic nano material preparation, and particularly relates to a rod-like / hexagonal flaky Co (OH) 2 nano composite structure and preparation and application thereof. In the prior art, the traditional synthesis method of the nano-structure Co (OH) 2 is a chemical precipitation method and an MOF template-based etching method, and the nano-structure Co (OH) 2 is mostly of a single sheet structure. Aiming at the phenomenon, the invention provides nano cobalt hydroxide with a rod-shaped / hexagonal sheet-shaped composite structure, which is obtained by adopting electrochemical reconstruction. The preparation method comprises the following steps: firstly, synthesizing conical Co (OH) 2 on a foamed nickel substrate, carrying out phosphating treatment on the conical Co (OH) 2 to obtain CoP, and then chemically depositing Co-MOF on foamed nickel / CoP to obtain foamed nickel / CoP / Co-MOF; and performing electrochemical scanning reconstruction to obtain the rod-like / hexagonal flaky cobalt hydroxide nano composite structure. The composite structure has excellent electrochemical performance in a supercapacitor as an electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic nano material preparation, and specifically relates to a rod-shaped / hexagonal sheet Co(OH)2 nano composite structure and preparation and application thereof. Background Art

[0002] Traditional fossil energy is non-renewable and the large-scale consumption of fossil energy will lead to environmental pollution. In addition, excessive consumption of fossil energy and large-scale emission of CO2 will cause ecological problems such as climate anomalies. In order to overcome the above energy and environmental ecological problems, researchers have successively developed new energy and energy storage devices including chemical energy, solar energy, wind energy, tidal energy, etc. In the current field of chemical energy storage devices, compared with lithium-ion batteries, supercapacitors have the advantages of fast charging and discharging, long cycle life and high energy density. The development of new electrode materials is a key step in the study of high-performance supercapacitors. At present, Co(OH)2 with different structures including nanoparticles, nanosheets, nanorods and nanotubes have been developed to achieve its high energy density storage. In order to further enhance the electrochemical activity of Co(OH)2, in addition to using chemical methods to regulate its micromorphology, constructing composite materials or composite structures is also a research idea to improve its electrochemical performance.

[0003] At present, the synthesis methods of Co(OH)2 nanosheets can be roughly divided into two types, one is the chemical precipitation method, and the other is the etching method based on the MOF template. In the chemical precipitation method, the patent CN104261489B reports a method for preparing hexagonal β-cobalt hydroxide nanosheets. Specifically, ethylene glycol, methanol and alkali are used to prepare a mixed solvent, and then a water-soluble cobalt salt and hydrazine hydrate are added to react, and finally a hexagonal β-cobalt hydroxide nanosheet is prepared. This product has excellent capacitance as a supercapacitor electrode. The patent with publication number CN106186085A reports a method for synthesizing hexagonal flaky cobalt hydroxide. First, a cobalt salt solution is prepared, and then a precipitant solution containing an alkali and a nitrogen-containing ligand is prepared, and the precipitant solution is added to the cobalt salt solution to undergo a precipitation reaction to generate a hexagonal flaky cobalt hydroxide. Both of these synthesis methods use a precipitant and a cobalt salt solution for precipitation reaction, and the hexagonal Co(OH)2 nanosheet can be controllably synthesized by changing the solvent system or the type of precipitant. In addition, Co(OH)2 nanosheets can be prepared by etching the MOF template. Patent CN114272945B reports a metal organic framework derived carbon growth cobalt hydroxide and its preparation method. Specifically, 2-methylimidazole zinc salt particles (ZIF-8) are heated in an inert gas to obtain nitrogen-doped porous carbon, and then the nitrogen-doped porous carbon is used as a template to grow Co(OH)2. In addition, patent CN115448376B reports a method for preparing cobalt-based nanosheets. Specifically, ZIF-67 material is used as a sacrificial template, and stable α-Co(OH)2 is finally synthesized by ion etching and in-situ growth of layered cobalt hydroxide at room temperature and stirring.

[0004] In summary, the traditional synthesis methods of nanostructured Co(OH)2 are chemical precipitation and etching based on MOF templates, and most of them are single sheet structures. There are few reports on the use of electrochemical methods to regulate the production of nanostructured Co(OH)2. Summary of the invention

[0005] In order to solve the problems existing in the field of controllable synthesis of existing nanostructured Co(OH)2, the present invention provides a rod-shaped / hexagonal sheet Co(OH)2 nanocomposite structure and a preparation method and application thereof.

[0006] The rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure of the present invention is composed of a rod-shaped structure with a rough surface and a hexagonal sheet-shaped structure with a smooth surface.

[0007] The preparation method of the rod-shaped / hexagonal sheet Co(OH)2 nanocomposite structure of the present invention comprises the following steps: firstly, a cone-shaped Co(OH)2 is synthesized on a nickel foam (NF) substrate, the cone-shaped Co(OH)2 is subjected to phosphating treatment to obtain nickel foam / CoP, and then Co-MOF is chemically deposited on the nickel foam / CoP to obtain a nickel foam / CoP / Co-MOF composite material. The composite material is used as a working electrode, and repeated electrochemical scanning is performed in an alkaline solution, and the electrochemical action is used to induce electrochemical reconstruction of the cone-shaped CoP and the Co-MOF block structure, and after electrochemical intervention under certain conditions, a rod-shaped / hexagonal sheet Co(OH)2 nanocomposite structure can be obtained.

[0008] The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure of the present invention comprises the following specific steps:

[0009] Step 1: Preparation of CoP: Synthesizing cone-shaped Co(OH)2 on a nickel foam (NF) substrate using cobalt salt by a hydrothermal synthesis method to obtain nickel foam / Co(OH)2, and then phosphating the obtained nickel foam / CoP;

[0010] Step 2: preparing CoP / Co-MOF: soaking the above nickel foam / CoP in an alcohol solution of cobalt salt and dimethylimidazole for a certain period of time to generate Co-MOF, thus obtaining nickel foam / CoP / Co-MOF;

[0011] Step 3: Electrochemical reconstruction of CoP / Co-MOF: The prepared nickel foam / CoP / Co-MOF is used as the working electrode, and the material is taken out after a certain period of electrochemical scanning by cyclic voltammetry in a strong alkaline solution of a certain concentration, and then washed with water, ethanol, and dried to obtain a rod-shaped / hexagonal sheet Co(OH)2 nanocomposite structure.

[0012] The phosphating treatment in step 1 is to put the phosphorus source powder and the foamed nickel / Co(OH)2 sample into a crucible in sequence, with the sample and the phosphorus source powder separated by about 3 cm, and perform thermal annealing to convert the foamed nickel / Co(OH)2 into foamed nickel / CoP;

[0013] The phosphorus source includes one of sodium dihydrogen hypophosphite and red phosphorus, or a mixture of the two in any proportion;

[0014] The annealing temperature is 200-300° C., and the annealing time is 1-5 hours.

[0015] The hydrothermal synthesis method in step 1 is to generate cone-shaped Co(OH)2 by hydrothermal reaction of cobalt salt in the presence of a precipitant, wherein the precipitant is urea or hexamethylenetetramine;

[0016] The reaction temperature of the hydrothermal synthesis method is 100-140° C., and the reaction time is 5-24 hours.

[0017] The cobalt salt in step 1 and step 2 includes one of cobalt nitrate, cobalt chloride, and cobalt sulfate, or a mixture of the above in any proportion; the alcohol in step 2 is an alcohol solvent, including methanol, isopropanol, etc., and the soaking time is 8 to 48 hours.

[0018] In step 3, the cyclic voltammetry scanning speed is 1 to 10 mV / s, and the number of repeated scanning cycles is 2 to 200 cycles; the strong alkaline solution is 1 to 6 mol / L KOH or NaOH solution.

[0019] The rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure of the present invention has excellent electrochemical performance as an electrode material in a supercapacitor.

[0020] Compared with the prior art, the characteristics and beneficial effects of the present invention are:

[0021] (1) The present invention uses a nickel foam / CoP / Co-MOF composite structure as a working electrode, and prepares a rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure through electrochemical induction in an alkaline electrolyte. The Co(OH)2 of the composite structure can integrate the fast ion transport characteristics of the rod-shaped structure and the highly active surface of the sheet structure. Compared with the traditional single-structure Co(OH)2, the composite structure is more conducive to improving the electrochemical activity and electrochemical performance of the electrode material.

[0022] (2) Compared with the existing chemical precipitation method and MOF template-based etching method, this electrochemical method can prepare hexagonal cobalt hydroxide nanosheets by regulating the number of electrochemical scans, thereby improving their electrochemical performance. In addition, the electrochemical method is not only used to in situ regulate the microstructure and composition of electrode materials, but also to monitor their electrochemical properties in real time, which is conducive to the preparation of electrode materials with better electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a microscopic morphology of the cone-shaped Co(OH)2 prepared by the hydrothermal method in Example 1 of the present invention;

[0024] Figure 2 This is a microscopic morphology of CoP / Co-MOF prepared by immersing nickel foam / CoP in cobalt salt in Example 1 of the present invention;

[0025] Figure 3 is an XRD pattern of the cobalt hydroxide nanocomposite structure prepared in Example 1 of the present invention;

[0026] Figure 4 is a microscopic morphology of the cobalt hydroxide nanocomposite structure prepared in Example 1 of the present invention;

[0027] Figure 5 is a microscopic morphology of the cobalt hydroxide nanocomposite structure prepared in Example 2 of the present invention;

[0028] Figure 6 is a microscopic morphology of the cobalt hydroxide nanocomposite structure prepared in Example 3 of the present invention;

[0029] Figure 7 is a microscopic morphology of the cobalt hydroxide nanocomposite structure prepared in Example 4 of the present invention;

[0030] Figure 8 This is a microscopic morphology of the cobalt hydroxide nanocomposite structure prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0031] The technical scheme of the present invention is clearly and completely described below in conjunction with the embodiments and the accompanying drawings. It should be pointed out that the embodiments described in the present invention are only used to further explain and illustrate, rather than to limit the scope of application. Based on the present invention, all other schemes obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0032] The electrode size in the embodiment is 1×1 cm 2 The nickel foam / CoP / Co-MOF prepared in each example was used as the working electrode, the platinum sheet was used as the counter electrode, and the reference electrode was the Hg / HgO electrode.

[0033] Example 1

[0034] Cobalt nitrate was used as cobalt salt for hydrothermal reaction, and cone-shaped Co(OH)2 was grown on the nickel foam substrate. The concentration of cobalt nitrate was 0.2 mol / L, the concentration of precipitant urea was 1 mol / L, the hydrothermal temperature was 100℃, and the reaction time was 5h to obtain nickel foam / Co(OH)2. Its microscopic morphology is shown in Figure 1 As shown, from Figure 1 It can be seen that the Co(OH)2 prepared by the hydrothermal method has a cone-shaped structure. CoP is prepared by phosphating treatment using thermal annealing. The phosphorus source used is 0.5g of sodium dihydrogen hypophosphite. The phosphorus source powder and the foamed nickel / Co(OH)2 sample are placed in a crucible in turn and the sample is 3cm to the right of the phosphorus source powder. The thermal annealing temperature is 200°C and the reaction time is 1h to obtain foamed nickel / CoP. The foamed nickel / CoP sample is immersed in a methanol solution of 0.1mol / L cobalt nitrate and 1.5mol / L dimethylimidazole for 48h to prepare CoP / Co-MOF, that is, a foamed nickel / CoP / Co-MOF sample is obtained. Its microscopic morphology is as follows Figure 2 As shown, from Figure 2It can be seen that CoP / Co-MOF is composed of cone-shaped and block-shaped structures. The above nickel foam / CoP / Co-MOF is used as the working electrode, the electrolyte is 1 mol / L NaOH solution, and the electrochemical scanning is performed by cyclic voltammetry at a scanning speed of 1 mV / s. After repeating the scanning for 6 times, a rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure can be prepared. The XRD pattern of the composite structure is shown in Figure 3 As shown in Figure 1, the characteristic peaks of the Co(OH)2 standard spectrum (PDF: 51-1731) are basically consistent, indicating that the rod-shaped / hexagonal sheet-shaped nanocomposite structure is composed of cobalt hydroxide. The microscopic morphology of the composite structure is shown in Figure 1. Figure 4 shown.

[0035] Example 2

[0036] Cobalt chloride was used as the cobalt salt for hydrothermal reaction, and cone-shaped Co(OH)2 was grown on the nickel foam substrate, wherein the concentration of cobalt chloride was 0.5 mol / L, the concentration of urea was 2 mol / L, the hydrothermal temperature was 120°C, and the reaction time was 10 h, to obtain nickel foam / Co(OH)2. CoP was prepared by phosphating treatment using thermal annealing, and the phosphorus source used was 0.2 g red phosphorus powder. The red phosphorus powder and the nickel foam / Co(OH)2 sample were placed in a crucible in turn, and the sample was 3 cm to the right of the red phosphorus powder. The thermal annealing temperature was 230°C, and the reaction time was 5 h, to obtain nickel foam / CoP. The nickel foam / CoP sample was immersed in a methanol solution of 0.5 mol / L cobalt sulfate and 2 mol / L dimethylimidazole for 24 h to prepare CoP / Co-MOF, that is, a nickel foam / CoP / Co-MOF sample was obtained. The nickel foam / CoP / Co-MOF was used as the working electrode, the electrolyte was 2 mol / L KOH solution, and the electrochemical scanning was performed by cyclic voltammetry at a scanning speed of 4 mV / s. After repeating the scanning for 20 cycles, a rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure was prepared. The microscopic morphology of the composite structure is shown in FIG. Figure 5 shown.

[0037] Example 3

[0038] Cobalt chloride was used as the cobalt salt for hydrothermal reaction, and cone-shaped Co(OH)2 was grown on the nickel foam substrate, wherein the concentration of cobalt chloride was 0.3 mol / L, the concentration of urea was 1.2 mol / L, the hydrothermal temperature was 140°C, and the reaction time was 24 h to obtain nickel foam / Co(OH)2. CoP was prepared by phosphating treatment using thermal annealing, and the phosphorus source used was 0.2 g red phosphorus powder. The red phosphorus powder and the nickel foam / Co(OH)2 sample were placed in a crucible in turn, and the sample was 3 cm to the right of the red phosphorus powder. The thermal annealing temperature was 250°C, and the reaction time was 2 h to obtain nickel foam / CoP. The nickel foam / CoP sample was immersed in a methanol solution of 0.8 mol / L cobalt chloride and 2.2 mol / L dimethylimidazole for 48 h to prepare CoP / Co-MOF, that is, a nickel foam / CoP / Co-MOF sample was obtained. The nickel foam / CoP / Co-MOF was used as the working electrode, the electrolyte was 5 mol / L NaOH solution, and the electrochemical scanning was performed by cyclic voltammetry at a scanning speed of 8 mV / s. After repeating the scanning for 200 times, a rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure was prepared. The microscopic morphology of the composite structure is shown in FIG. Figure 6 shown.

[0039] Example 4

[0040] Cobalt sulfate and cobalt chloride were used as cobalt salts for hydrothermal reaction, and cone-shaped Co(OH)2 was grown on the nickel foam substrate, where the concentration of cobalt sulfate was 0.2 mol / L, the concentration of cobalt chloride was 0.1 mol / L, the concentration of hexamethylenetetramine was 1.5 mol / L, the hydrothermal temperature was 130°C, and the reaction time was 16 h to obtain nickel foam / Co(OH)2. CoP was prepared by phosphating by thermal annealing, and the phosphorus source used was 0.1 g red phosphorus powder and 0.1 g sodium dihydrogen hypophosphite. The mixed phosphorus source powder and nickel foam / Co(OH)2 sample were placed in a crucible in turn, and the sample was 3 cm to the right of the powder. The thermal annealing temperature was 240°C, and the reaction time was 2.5 h to obtain nickel foam / CoP. The nickel foam / CoP sample was immersed in an isopropanol solution of 1 mol / L cobalt sulfate and 3 mol / L dimethylimidazole for 36 hours to prepare CoP / Co-MOF, that is, a nickel foam / CoP / Co-MOF sample was obtained. The nickel foam / CoP / Co-MOF was used as a working electrode, the electrolyte was a 6 mol / L KOH solution, and cyclic voltammetry was used for electrochemical scanning at a scanning speed of 10 mV / s. After repeating the scanning for 110 times, a rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure was prepared. The microscopic morphology of the composite structure is shown in FIG. Figure 7 shown.

[0041] Example 5

[0042] Cobalt nitrate, cobalt sulfate and cobalt chloride were used as cobalt salts for hydrothermal reaction, and cone-shaped Co(OH)2 was grown on the nickel foam substrate, wherein the concentration of cobalt nitrate was 0.1 mol / L, the concentration of cobalt sulfate was 0.1 mol / L, the concentration of cobalt chloride was 0.1 mol / L, the concentration of hexamethylenetetramine was 2 mol / L, the hydrothermal temperature was 110°C, the reaction time was 9 hours, and nickel foam / Co(OH)2 was obtained. CoP was prepared by phosphating treatment using thermal annealing, and the phosphorus source used was 0.2 g red phosphorus powder. The red phosphorus powder and nickel foam / Co(OH)2 samples were placed in a crucible in turn, and the sample was 3 cm to the right of the red phosphorus powder. The thermal annealing temperature was 220°C, and the reaction time was 2 hours, and nickel foam / CoP was obtained. The nickel foam / CoP sample was immersed in an isopropanol solution of 1.2 mol / L cobalt chloride and 3.2 mol / L dimethylimidazole for 36 hours to prepare CoP / Co-MOF, that is, a nickel foam / CoP / Co-MOF sample was obtained. The nickel foam / CoP / Co-MOF was used as a working electrode, the electrolyte was a 2 mol / L KOH solution, and cyclic voltammetry was used for electrochemical scanning at a scanning speed of 2 mV / s. After repeating the scanning for 70 times, a rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure was prepared. The microscopic morphology of the composite structure is shown in FIG. Figure 8 shown.

[0043] from Figures 4 to 8 It can be seen that the rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structures prepared in the present invention are composed of a rod-shaped structure with a rough surface and a hexagonal sheet-shaped structure with a smooth surface.

[0044] Table 1 lists the specific capacitance data of different samples calculated according to the discharge time at a current density of 1A / g after constant current charge and discharge tests using a three-electrode system. By comparison, it is found that the specific capacitance of the rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure prepared by the electrochemical reconstruction process is higher than that of the initially synthesized cone-shaped cobalt hydroxide and the CoP / Co-MOF sample before reconstruction, which proves that the rod-shaped / hexagonal sheet-shaped cobalt hydroxide nanocomposite structure prepared after electrochemical reconstruction has better electrochemical performance. The reason for the performance improvement depends on the synergistic effect of the rough rod-shaped structure and the hexagonal sheet structure, in which the rod-shaped structure has the characteristics of rapid ion transmission, and the hexagonal sheet structure can provide a highly active surface.

[0045] Table 1 Specific capacitance test values ​​of cone-shaped Co(OH)2, CoP / Co-MOF and rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structures prepared by hydrothermal method

[0046] Example 1 Example 2 Example 3 Example 4 Example 5 <![CDATA[Cone-shaped Co(OH)2]]> 996F / g 1232F / g 1035F / g 1132F / g 1205F / g CoP / Co-MOF 1321F / g 1453F / g 1542F / g 1316F / g 1469F / g <![CDATA[Co(OH)2 composite structure]]> 2450F / g 2210F / g 2635F / g 2317F / g 2478F / g .

Claims

1. A rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure, characterized in that: The composite structure consists of a rod-like structure with a rough surface and a hexagonal sheet-like structure with a smooth surface.

2. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 1, characterized in that: Includes the following methods: Firstly, conical Co(OH)2 is synthesized on a nickel foam substrate, and the conical Co(OH)2 is phosphated to obtain nickel foam / CoP. Then, Co-MOF is chemically deposited on the nickel foam / CoP to obtain nickel foam / CoP / Co-MOF. The nickel foam / CoP / Co-MOF is used as a working electrode and electrochemical scanning is carried out in an alkaline solution to electrochemically reconstruct the conical CoP and Co-MOF block structures to obtain a rod-shaped / hexagonal sheet Co(OH)2 nanocomposite structure.

3. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 2, characterized in that: The specific steps include: Step 1: preparing CoP: using a hydrothermal synthesis method to synthesize cone-shaped Co(OH)2 on a nickel foam substrate using cobalt salt to obtain nickel foam / Co(OH)2, and then phosphating the obtained nickel foam / CoP; Step 2: preparing CoP / Co-MOF: soaking the above nickel foam / CoP in an alcohol solution of cobalt salt and dimethylimidazole to generate CoP / Co-MOF, that is, obtaining nickel foam / CoP / Co-MOF; Step 3: Electrochemical reconstruction of CoP / Co-MOF: The nickel foam / CoP / Co-MOF prepared above was used as the working electrode, and electrochemical scanning was performed by cyclic voltammetry in a strong alkaline solution to obtain a rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure.

4. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 3, characterized in that: The phosphating treatment in step 1 is to place the phosphorus source powder and the foamed nickel / Co(OH)2 sample in a crucible with a distance of 3 cm between the sample and the phosphorus source powder, and perform thermal annealing to convert the foamed nickel / Co(OH)2 into foamed nickel / CoP.

5. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 4, characterized in that: In step 1, the phosphorus source includes sodium dihydrogen hypophosphite, red phosphorus, or a mixture of the two in any proportion; the annealing temperature is 200-300° C., and the annealing time is 1-5 hours.

6. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 3, characterized in that: The hydrothermal synthesis method described in step 1 is to generate conical Co(OH)2 by hydrothermal reaction of cobalt salt in the presence of a precipitant, wherein the precipitant is urea or hexamethylenetetramine.

7. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 3, characterized in that: The reaction temperature of the hydrothermal synthesis method in step 1 is 100-140° C., and the reaction time is 5-24 hours.

8. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 3, characterized in that: The cobalt salt in step 1 and step 2 includes one of cobalt nitrate, cobalt chloride, and cobalt sulfate, or a mixture of the above in any proportion; the alcohol in step 2 is an alcohol solvent, including methanol and isopropanol, and the soaking time is 8 to 48 hours.

9. The method for preparing the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 3, characterized in that: In step 3, the cyclic voltammetry scanning speed is 1 to 10 mV / s, and the number of repeated scanning cycles is 2 to 200 cycles; the strong alkaline solution is 1 to 6 mol / L KOH or NaOH solution.

10. The use of the rod-shaped / hexagonal sheet-shaped Co(OH)2 nanocomposite structure according to claim 1, characterized in that: The cobalt hydroxide nanocomposite structure is used as an electrode material for supercapacitors.