Ultrasonic electrolysis method for efficiently preparing high-purity indium

By introducing ultrasonic accelerated particles to diffusion and precipitation during the electrolysis process, the problem of long-term and low efficiency of traditional electrolysis methods is solved, and the rapid and efficient preparation of high-purity indium of 99.999% purity is achieved, improving the electrolytic efficiency and purity.

CN118979285APending Publication Date: 2024-11-19GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411109306.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Traditional electrolysis methods are used to purify high-purity indium for a long time and low efficiency, making it difficult to quickly generate high-purity indium elements.

Method used

Ultrasonic waves are introduced during the electrolysis process, and particles are accelerated through an ultrasonic system with a frequency of 40kHz to improve electrolysis efficiency. The electrolyte and indium electrode groups of specific ratios are used to perform DC repeated electrolysis, and remelting at high temperatures is achieved with a high of 99.999% Pure indium.

Benefits of technology

It realizes the rapid batch generation of 5N high-purity indium, significantly shortens the preparation time, improves the electrolytic efficiency, and ensures the production of high-purity indium elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979285A_ABST
    Figure CN118979285A_ABST
Patent Text Reader

Abstract

The invention provides an ultrasonic electrolysis method for efficiently preparing high-purity indium. According to the ultrasonic electrolysis method, the high-purity indium with the purity reaching 99.999% is obtained according to the first step of electrolyte proportioning, the second step of indium electrode plate manufacturing, the third step of ultrasonic system installation, the fourth step of repeated electrolysis and the fifth step of remelting. According to the method, ultrasonic waves are introduced into electrolytic indium, under the action of the ultrasonic waves, the electrolyte can continuously scour an indium anode plate, particles are accelerated to be separated from the anode plate, the electrolyte can be activated, particle diffusion can be accelerated, indium particles in the electrolyte can be further evenly distributed, and the electrochemical performance of the electrolyte is improved. And precipitation and deposition of indium particles are accelerated, so that the electrolysis efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an ultrasonic electrolysis method for efficiently preparing high-purity indium, belonging to the technical field of purification, and mainly accelerates particle diffusion and precipitation by introducing ultrasonic waves to improve the electrolysis efficiency of high-purity indium. Background Art

[0002] High-purity indium is a single element of indium with a purity of 99.999%. It has many important applications. High-purity indium is mainly used to make semiconductor compounds, high-purity alloys and dopants for semiconductor materials. Its physical properties include a silvery-white metallic appearance, soft texture, and excellent ductility and plasticity. The density of high-purity indium is 7.31g / cm³ and the melting point is 156.2℃. In the military and aerospace fields, high-purity indium is used to manufacture lnAs infrared detectors and stealth materials; in the semiconductor industry, high-purity indium is used as electrodes and crystal growth materials in the manufacture of compound semiconductor materials; in the optical industry, high-purity indium is used to manufacture optical components such as photovoltaic films and reflectors.

[0003] High-purity indium is hailed as "the irreplaceable raw material for the world's fourth scientific and technological revolution", but the traditional electrolysis method for purifying high-purity indium takes a long time and has low efficiency. Therefore, we proposed the ultrasonic electrolysis method, which can accelerate the diffusion and precipitation of particles and improve the electrolysis efficiency. Summary of the invention

[0004] The present invention provides an ultrasonic electrolysis method for efficiently preparing high-purity indium. The method mainly accelerates particle diffusion and precipitation by introducing ultrasonic waves during electrolysis, thereby enabling rapid batch production of 5N grade (99.999%) high-purity indium, effectively solving the problem of long time and low efficiency of traditional electrolysis.

[0005] One of the technical solutions of the present invention is achieved by the following measures: an ultrasonic electrolysis method for efficiently preparing high-purity indium, characterized in that it is carried out according to the following steps: Step 1: Prepare an electrolyte by mixing and adding the electrolyte into a glass electrolytic cell. The electrolyte is prepared by adding 70-90 g / L of indium with a purity of 99%, 0.3 g / L of gelatin, and 60-100 g / L of sodium chloride into a dilute sulfuric acid solution with a volume concentration of 15%-20%. Step 2: Make indium electrode plates with a purity of 99%, one as an indium anode plate and the other as an indium cathode plate, and use the two indium anode plates and the indium cathode plate as an indium electrode group; insert multiple groups of indium electrode groups into the electrolyte; Step 3: Install an ultrasonic system in the electrolysis system and maintain the ultrasonic frequency at 40kHz and the power at 4kw; Step 4: Direct current is passed through the indium electrode group for repeated electrolysis 3 times, and the current density is 40-60A / m2 , the temperature of the whole process is kept at about 20℃; Step 5: After repeated electrolysis for 3 times, take out the indium cathode plate, scrape off the indium crystals on the plate, and then remelt it at 180℃-250℃ to obtain high-purity indium with a purity of 99.999% (5N).

[0006] It is further explained that the ultrasonic system will generate ultrasonic waves with a frequency of 40kHz. Under the action of ultrasonic waves, the electrolyte will continuously flush the indium anode plate, accelerating the particles to detach from the anode plate, diffuse, and precipitate.

[0007] The ultrasonic electrolysis method for efficiently preparing high-purity indium of the present invention introduces ultrasonic waves into the electrolytic indium. Under the action of ultrasonic waves, the electrolyte will continuously flush the indium anode plate, accelerate the separation of particles from the anode plate, activate the electrolyte, and accelerate the diffusion of particles, further make the indium particles in the electrolyte evenly distributed, and accelerate the precipitation and deposition of indium particles to accelerate the efficiency of electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Attached Figure 1 The present invention is a schematic structural diagram of an ultrasonic electrolysis method for efficiently preparing high-purity indium. DETAILED DESCRIPTION

[0009] The present invention is not limited by the following embodiments, and specific implementation methods can be determined according to the technical solution of the present invention and actual conditions. The present invention is further described below in conjunction with the embodiments: Implementation Case 1 In a dilute sulfuric acid solution with a volume concentration of 15%, 70 g / L of indium with a purity of 99%, 0.3 g / L of gelatin, and 60 g / L of sodium chloride are added to obtain an electrolyte, and the electrolyte is added to an electrolytic cell made of glass; Then, indium with a purity of 99% is made into indium electrode plates, one as an indium anode plate and the other as an indium cathode plate, and the two indium anode plates and the indium cathode plate are used as an indium electrode group; two groups of indium electrode groups are inserted into the electrolyte; Next, an ultrasonic system is installed in the electrolysis system, and the ultrasonic frequency is maintained at 40kHz and the power is 4kw; Direct current was passed through the indium electrode group and electrolysis was repeated three times with a current density of 40 A / m 2 , the temperature of the whole process was kept at 18℃; After repeated electrolysis three times, the indium cathode plate was taken out, and finally the indium crystals on the plate were scraped off and remelted at 200°C to obtain indium. After testing, the purity was found to be 99.9991%.

[0010] Implementation Case 2 In a dilute sulfuric acid solution with a volume concentration of 20%, 90 g / L of indium with a purity of 99%, 0.3 g / L of gelatin, and 100 g / L of sodium chloride are added to obtain an electrolyte, and the electrolyte is added to an electrolytic cell made of glass; Then, indium with a purity of 99% is made into indium electrode plates, one as an indium anode plate and the other as an indium cathode plate. The two indium anode plates and the indium cathode plate are used as an indium electrode group; three groups of indium electrode groups are inserted into the electrolyte; Next, an ultrasonic system is installed in the electrolysis system, and the ultrasonic frequency is maintained at 40kHz and the power is 4kw; Direct current was passed through the indium electrode group and electrolysis was repeated three times with a current density of 60 A / m 2 , the temperature of the whole process was kept at 25℃; After repeated electrolysis three times, the indium cathode plate was taken out, and finally the indium crystals on the plate were scraped off and remelted at 250°C to obtain indium. After testing, the purity was found to be 99.9993%.

Claims

1. An ultrasonic electrolysis method for efficiently preparing high-purity indium, characterized in that Follow these steps: Step 1: Prepare an electrolyte by mixing and adding the electrolyte into a glass electrolytic cell. The electrolyte is prepared by adding 70-90 g / L of indium with a purity of 99%, 0.3 g / L of gelatin, and 60-100 g / L of sodium chloride into a dilute sulfuric acid solution with a volume concentration of 15%-20%. Step 2: Make indium electrode plates with a purity of 99%, one as an indium anode plate and the other as an indium cathode plate, and use the two indium anode plates and the indium cathode plate as an indium electrode group; insert multiple groups of indium electrode groups into the electrolyte; Step 3: Install an ultrasonic system in the electrolysis system and maintain the ultrasonic frequency at 40kHz and the power at 4kw; Step 4: Direct current is passed through the indium electrode group for repeated electrolysis 3 times, and the current density is 40-60A / m 2 , the temperature of the whole process is kept at about 20℃; Step 5: After repeated electrolysis for 3 times, take out the indium cathode plate, scrape off the indium crystals on the plate, and then remelt it at 180℃-250℃ to obtain high-purity indium with a purity of 99.999% (5N).

2. According to claim 1, an ultrasonic electrolysis method for efficiently preparing high-purity indium, characterized in that: The ultrasonic system generates ultrasonic waves with a frequency of 40kHz. Under the action of ultrasonic waves, the electrolyte will continuously flush the indium anode plate, accelerating the particles to detach from the anode plate, diffuse, and precipitate.